A synthetic cement raw material additive and its preparation method and application

By using a combination of synthetic organic acid salts, organic esters and high-efficiency diffusing agents, cement raw meal additives are prepared, which solves the problems of uncertain usage amounts and unstable effects of cement raw meal additives in the existing technology, and achieves high-efficiency powder Grinding and improving the calcination performance of cement raw meal, significantly improving cement grinding efficiency and clinker quality.

CN116282990BActive Publication Date: 2024-10-29鲁昌宝
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310262856.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-29
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

The usage amount of existing cement raw meal additives cannot be determined and the effect is unstable. It is impossible to improve cement grinding efficiency and calcination performance at the same time, and the existing technology cannot guarantee that raw meal additives can effectively improve the quality of cement clinker.

Method used

Synthetic organic acid salts, synthetic organic esters and high-efficiency diffusing agents (such as the combination of nano-light diffusing agent JSY-168 and sodium dodecyl sulfate) are used as raw materials, and cement raw material additives are prepared through stirring and temperature control to ensure that each The components are evenly distributed and dispersed, reducing the viscosity and improving the grinding efficiency and burnability.

Benefits of technology

It significantly improves the grinding efficiency of cement raw meal, reduces grinding energy consumption, improves the burnability of cement raw meal, and ensures the improvement of clinker quality. The effect is better than the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004131925360000091
    Figure BDA0004131925360000091
  • Figure BDA0004131925360000111
    Figure BDA0004131925360000111
  • Figure BDA0004131925360000112
    Figure BDA0004131925360000112
Patent Text Reader

Abstract

The invention relates to the technical field of cement additives, and more specifically, to a synthetic cement raw material additive and a preparation method and application thereof. The cement raw material additive is composed of the following raw materials in percentage by mass: 15-40% of a synthetic organic acid salt, 12-28% of a synthetic organic ester, 2-9% of a high-efficiency diffuser, and the balance is supplemented by deionized water. The preparation method of the synthetic cement raw material additive comprises the following steps: (1) synthesizing an organic acid salt in a reaction kettle; (2) synthesizing an organic ester in a reaction kettle; (3) adding the synthetic organic acid salt, the synthetic organic ester, the high-efficiency diffuser, and deionized water into the reaction kettle, stirring at a speed of 50-80 r / min for 10-30 min, then controlling the temperature at 60-80 DEG C, stirring at a speed of 80-120 r / min, reacting for 30-50 min, and cooling to obtain the synthetic cement raw material additive; the synthetic cement raw material additive is added at a raw material preparation warehouse before the new dry process cement raw material enters a mill, and is accurately metered and added according to the designed mixing amount using a special additive metering pump. The prepared cement raw meal additive can significantly reduce the 80μm and 200μm sieve residues of the raw meal, improve the grinding efficiency of the cement raw meal, reduce the grinding energy consumption and improve the burnability of the cement raw meal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cement additives, in particular to the field of IPC C04, and more specifically to a synthetic cement raw material additive and a preparation method and application thereof. Background Art

[0002] Cement is one of the most important basic raw materials in building materials. The process of cement production includes the production links of "two grindings and one burning", namely raw material grinding, kiln calcination, and clinker grinding. The raw materials are mainly lime, clay, mineralizers, and correction raw materials. According to a specific ratio, they are crushed, ground, and mixed into cement raw materials. Since the raw material particles of cement raw materials are large and the particle size is uneven, an appropriate amount of cement grinding aids can be added during the grinding process to improve the grinding efficiency. Adding cement raw material aids can effectively improve the fluidity of cement raw materials, thereby improving the effect and performance of cement grinding and reducing the energy consumption of cement raw material grinding. As a process aid in the processing of cement raw materials, cement raw material aids can also significantly improve the mixing uniformity of each raw material particle, stimulate the hydration activity of each mixed raw material, and thus improve the use intensity of cement at each age. At the same time, by reducing the coarse particle content, improving the structure of ore materials, and increasing the high-temperature reaction activity of raw material components in the cement raw material grinding stage, the burnability of cement raw materials can be effectively improved, thereby reducing the energy consumption of subsequent clinker burning.

[0003] At present, most of the existing cement raw material additives are directly purchased chemical waste liquids, or are simply mixed and prepared using industrial raw materials, resulting in the inability to determine the amount of cement raw material additives used and unstable effects. CN114477844B discloses a cement raw material grinding aid and its preparation method and application. The cement raw material grinding aid provided by the invention is prepared from the following components in percentage by weight: 10-25% organic acid salt; 11%-24% polymer ester; 9-16% polyol; 2%-5% rare earth stabilizer; 45%-60% deionized water. The prepared cement raw material grinding aid can reduce the grinding energy consumption and reduce the coal consumption of clinker burning, but its performance is insufficient. In actual use, the required addition amount of cement raw material grinding aid is relatively high; CN113800796A discloses a cement raw material aid and a preparation method thereof, wherein the raw material composition comprises: 10-17% of raw material decomposition promoter, 13-16% of coal saving agent, 6-9% of grinding aid enhancer, 10-14% of desulfurization activator, and 0.1-0.3% of dispersant; the balance is water, and the total amount is 100%. It has good energy-saving and coal-saving, production-increasing and enhancing effects, and the effect is long-lasting and high-temperature resistant, and the liquid is more convenient to use, and has a more environmentally friendly desulfurization effect, but it cannot guarantee that the prepared raw material aid can effectively improve the quality of cement clinker at the same time. Therefore, the development of cement raw material aids that can not only significantly improve the grinding efficiency of cement raw materials, but also effectively improve the calcination performance of cement raw materials with cement additives added, and ensure the quality of cement clinker is the current development direction. Summary of the invention

[0004] In order to solve the above problems, the first aspect of the present invention provides a synthetic cement raw material additive, which includes, by mass percentage, 15-40% synthetic organic acid salt, 12-28% synthetic organic ester, 2-9% high-efficiency diffusant, and deionized water to make up the balance.

[0005] Preferably, the raw materials of the synthetic cement raw material additive include, by mass percentage: 18-35% of synthetic organic acid salt, 15-25% of synthetic organic ester, 3-7% of high-efficiency diffusant, and deionized water to make up the balance.

[0006] Preferably, the raw materials of the synthetic cement raw material additive include, by mass percentage: 30% synthetic organic acid salt, 18% synthetic organic ester, 5% high-efficiency diffusant, and the balance made up by deionized water.

[0007] Preferably, the high-efficiency diffusing agent is at least one of a light diffusing agent, an inorganic dispersant, and an organic dispersant.

[0008] Preferably, the high-efficiency diffuser is a combination of a nano light diffuser and an organic dispersant.

[0009] Preferably, the mass ratio of the nano light diffuser to the organic dispersant is (0.1-5):(0.5-4).

[0010] Preferably, the mass ratio of the nano light diffuser to the organic dispersant is (0.5-2):(1-3).

[0011] Preferably, the mass ratio of the nano light diffuser to the organic dispersant is 1:2.

[0012] Preferably, the nano light diffuser is at least one of nano barium sulfate and nano organosilicon light diffuser.

[0013] Preferably, the nano light diffuser is nano light diffuser JSY-168.

[0014] Preferably, the organic dispersant is at least one of triethylhexyl phosphate, sodium lauryl sulfate, methylpentanol, polyacrylamide, and fatty acid polyethylene glycol ester.

[0015] Preferably, the organic dispersant is sodium dodecyl sulfate.

[0016] Preferably, the high-efficiency diffuser is a composition of nano light diffuser JSY-168 and sodium dodecyl sulfate, and the mass ratio of the composition of nano light diffuser JSY-168 and sodium dodecyl sulfate is 1:2.

[0017] The present application uses a combination of nano light diffuser JSY-168 and sodium dodecyl sulfate as a high-efficiency diffuser, which can improve the dispersion of synthetic organic acid salts and synthetic organic esters in the prepared product, so that the components of the system are evenly distributed, and the components are prevented from aggregating and stratifying, thereby causing cement segregation. In particular, when the mass ratio of nano light diffuser JSY-168 to sodium dodecyl sulfate is 1:2, the dispersibility of the components in the system can be further improved, and the viscosity of the cement raw material additive can be reduced. The critical micelle concentration of sodium dodecyl sulfate is low, and the generated mixed additive emulsion particles are smaller, the mechanical stability is better, and the agglomeration phenomenon is less; the nano light diffuser JSY-168 has a silicon-oxygen bond and a three-dimensional microsphere structure. After being added into the system, it is evenly distributed in the system in the form of a fine glass sphere structure, and can improve the stability of particles in the system through the action of silicon-oxygen bonds and other chemical bonds. The two are compounded in this ratio, and after the dispersion degree of substances in the system is improved by sodium dodecyl sulfate, the nano light diffuser JSY-168 strengthens the dispersion stability between the particles, and at the same time makes the components evenly and stably dispersed in the system play a filling role in the cement raw material grinding process, which is beneficial for the cement raw material additive to reduce the fracture energy barrier of mineral raw materials such as limestone and minerals, and reduce the mineral reaction activation energy in the clinker calcination process, thereby improving the cement raw material additive to improve the grinding efficiency of cement raw materials, reduce grinding energy consumption and improve the burnability of cement raw materials.

[0018] A second aspect of the present invention provides a method for preparing the synthetic cement raw material additive as described above, comprising the following steps:

[0019] (1) preparing a synthetic organic acid salt in a reaction kettle; (2) preparing a synthetic organic ester in a reaction kettle; (3) adding the synthetic organic acid salt, the synthetic organic ester, the high-efficiency dispersant and deionized water into the reaction kettle, stirring at a speed of 50 to 80 r / min for 10 to 30 min, then controlling the temperature at 60 to 80° C., stirring at a speed of 80 to 120 r / min, reacting for 30 to 50 min, and cooling to obtain the product.

[0020] Preferably, the specific method of step (3) is: adding synthetic organic acid salt, synthetic organic ester, high-efficiency diffusant and deionized water into a reaction kettle, stirring at a speed of 60 r / min for 15 min, then controlling the temperature at 70° C., stirring at a speed of 100 r / min, reacting for 40 min, and cooling to obtain the product.

[0021] Preferably, the specific method of step (1) is: adding 20-40% alkaline inorganic solution and organic acid into a reaction kettle, controlling the temperature at 60-80°C, stirring at a speed of 45-55 r / min for 30-50 minutes, and obtaining the synthesized organic acid salt.

[0022] Preferably, the specific method of step (1) is: adding 30% alkaline inorganic solution and organic acid into a reaction kettle, controlling the temperature to 70° C., stirring at a speed of 55 r / min for 40 minutes, and obtaining the synthesized organic acid salt.

[0023] Preferably, the specific method of step (2) is: add 15-32% alkaline inorganic solution and organic polyol into a reaction kettle, control the temperature at 63-78°C, stir and react at a speed of 40-60 r / min for 30-50 minutes, and obtain the synthesized organic ester.

[0024] Preferably, the specific method of step (2) is: adding 24% alkaline inorganic solution and organic polyol into a reaction kettle, controlling the temperature to 70° C., stirring at a speed of 50 r / min for 40 minutes, and obtaining the synthesized organic ester.

[0025] Preferably, the organic acid is at least one of formic acid, acetic acid, propionic acid, butyric acid, phthalic acid, adipic acid, benzoic acid, salicylic acid, caffeic acid, citric acid, oxalic acid, tartaric acid, and succinic acid.

[0026] Preferably, the organic acid is at least one of formic acid, acetic acid, propionic acid, butyric acid, phthalic acid, and adipic acid.

[0027] Preferably, the organic polyol is at least one of pentaerythritol, ethylene glycol, 1,2-propylene glycol, propylene glycol, butylene glycol, 1,4-butylene glycol, 1,6-hexanediol, propylene glycol, neopentyl glycol, diethyl ether, trimethylolpropane, and glycerol.

[0028] Preferably, the organic polyol is at least one of ethylene glycol, propylene glycol, butylene glycol, dipropylene glycol, trimethylolpropane and glycerol.

[0029] The third aspect of the present invention provides an application of the synthetic cement raw material additive as described above, wherein the synthetic cement raw material additive is added at the raw material blending warehouse before the new dry process cement raw material enters the mill, and is accurately metered and added according to the designed addition amount using a special additive metering pump.

[0030] Preferably, the amount of the synthetic cement raw material additive added is 0.7‰ to 1.1‰ of the total mass.

[0031] Preferably, the amount of the synthetic cement raw material additive added is 0.9‰.

[0032] Beneficial effects:

[0033] 1. The organic acid salt synthesized in the present application is a surfactant, not a single species. The metal ions formed after dissolving in water have little effect in the raw material grinding process, but have the effect of increasing the liquid phase amount and reducing the liquid phase viscosity in the clinker calcination process; the anionic groups are directionally adsorbed on the surface of the microcracks of the material, which can promote the structural destruction of the particles on the one hand to achieve their refinement, thereby reducing the 80μm and 200μm sieve residues of the raw material; on the other hand, the microcrack surface adsorbed with polar anionic groups has a neutralization effect of static charge, which greatly weakens the crack healing tendency, helps to improve its high-temperature reaction activity, reduce the thermodynamic reaction activation energy, and increase the kinetic high-temperature solid-phase reaction rate, thereby improving its susceptibility to burn.

[0034] 2. The organic ester synthesized in this application is a surfactant with good wetting effect. It can effectively avoid the adsorption and agglomeration of fine limestone (or silica) particles in cement raw materials, improve the effective power of grinding, and help the overall particle size of raw materials to be finer, thereby effectively reducing the phenomenon of over-grinding and effectively reducing the waste of grinding energy. At the same time, the synthetic organic ester will release its own heat at high temperature in the cement kiln, which can help the burning rate of clinker and appropriately reduce the amount of coal used.

[0035] 3. In the present application, by using the nano light diffuser JSY-168 and sodium dodecyl sulfate as a high-efficiency diffuser, the dispersion degree of the synthetic organic acid salt and the synthetic organic ester in the prepared product can be improved, so that the components of the system are evenly distributed, and the components are prevented from aggregating and stratifying. After the dispersion degree of the substances in the system is improved by sodium dodecyl sulfate, the nano light diffuser JSY-168 enhances the dispersion stability between the particles, and at the same time, the components evenly and stably dispersed in the system play a filling role in the cement raw material grinding process, which is beneficial for the cement raw material additive to reduce the fracture energy barrier of mineral raw materials such as limestone and minerals, reduce the mineral reaction activation energy during the clinker calcination process, promote the structural destruction of the particles to achieve their refinement, thereby reducing the 80μm and 200μm sieve residues of the raw material. The synthetic cement raw material additive prepared in the present application is significantly higher than the existing technology level in terms of improving the grinding efficiency of cement raw materials, reducing grinding energy consumption and improving the burnability of cement raw materials.

[0036] 4. The synthetic cement additive carrier used in this application is deionized water from which cations and anions have been removed in advance. Tap water or river water cannot be used directly to prevent the large amount of ions contained therein from reacting with the components in the additive during stirring in the reactor, causing a variety of complex chemical reactions and forming corresponding impurities, thereby affecting the quality of the additive product. DETAILED DESCRIPTION

[0037] Example

[0038] Example 1 provides a synthetic cement raw material additive, the raw materials of which include, by mass percentage, 30% of synthetic organic acid salt, 18% of synthetic organic ester, 5% of high-efficiency diffusant, and the balance made up of deionized water.

[0039] The preparation method of the synthetic cement raw material additive comprises the following steps:

[0040] (1) Add 80 g of 30% alkaline inorganic aqueous solution and 35 g of organic acid into a reaction kettle, control the temperature to 70° C., stir at a speed of 55 r / min for 40 min, and obtain a synthetic organic acid salt;

[0041] (2) Add 60g of 24% alkaline inorganic aqueous solution and 19g of organic polyol into a reaction kettle, control the temperature to 70°C, stir at 50r / min for 40min, and obtain synthetic organic ester; (3) Add synthetic organic acid salt, synthetic organic ester, high-efficiency diffusant, and deionized water into a reaction kettle according to mass percentage, stir at 60r / min for 15min, then control the temperature to 70°C, stir at 100r / min, react for 40min, and cool to obtain.

[0042] The alkaline inorganic aqueous solution is a sodium hydroxide aqueous solution; the organic acid is a mixture of formic acid, acetic acid, butyric acid and phthalic acid, and the mass ratio of formic acid, acetic acid, butyric acid and phthalic acid is 1:2:1.5; the organic polyol is a mixture of ethylene glycol, propylene glycol and butylene glycol, and the mass ratio of ethylene glycol, propylene glycol and butylene glycol is 1:0.8:1.3.

[0043] Formic acid (CAS No.: 64-18-6), acetic acid (CAS No.: 64-19-7), phthalic acid (CAS No.: 100-21-0), and ethylene glycol (CAS No.: 107-21-1) were purchased from Shanghai En Chemical Technology Co., Ltd.

[0044] Propylene glycol (CAS No.: 57-55-6) was purchased from Beijing Bailingwei Technology Co., Ltd.

[0045] Butanediol (CAS No.: 4208-57-5) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0046] The high-efficiency diffuser is a composition of nano light diffuser JSY-168 and sodium dodecyl sulfate, and the mass ratio of the composition of nano light diffuser JSY-168 and sodium dodecyl sulfate is 1:2.

[0047] Nano light diffuser JSY-168 was purchased from Qianhai Jishengya (Shenzhen) Technology Co., Ltd.

[0048] Sodium dodecyl sulfate (CAS No.: 151-21-3) was purchased from Shanghai Yien Chemical Technology Co., Ltd.

[0049] The synthetic cement raw material additive as mentioned above is added at the raw material preparation warehouse before the new dry process cement raw material enters the mill, and is added with precise metering according to the designed mixing mass ratio of 0.9‰ using a special additive metering pump.

[0050] Performance Test:

[0051] Cement raw meal fineness test method sieve analysis method refer to GB / T 1345-2005;

[0052] The determination method of f-CaO content in clinker shall refer to GB / T 176-2008;

[0053] The test methods for cement standard consistency water consumption, setting time and stability refer to GB / T1346-2005;

[0054] The test standard for fluidity of cement mortar refers to GB / T 2419-2005;

[0055] The test method for cement mortar strength refers to GB / T 17671-1999;

[0056] Cement raw material particle gradation test refers to JC / T721-2006;

[0057] The test on the calcinability of cement raw materials refers to GB / T26566-2011;

[0058] The calorific value of coal is determined by oxygen-nitrogen method according to GB / T26566-2011.

[0059] Performance Test 1:

[0060] (1) The mass ratio of cement raw materials is: limestone: high silicon: ash: shale = 85.3:6.2:2.6:5.9.

[0061] (2) After 11 minutes of mixing according to the above cement raw material mix ratio, the blank sample is sample number A0;

[0062] (3) Add 0.15% of commercially available CD cement raw material additive into cement raw material and grind for 11 min, which is recorded as sample number A1;

[0063] (4) Add HX-SZY-I type cement raw material additive to cement raw material at a dosage of 0.12%, grind for 11 minutes, and record it as sample number A2;

[0064] (5) The cement raw material additive product synthesized in Example 1 was added to the cement raw material at an addition amount of 0.9‰ and ground for 11 minutes. The parallel test was conducted three times and recorded as sample numbers A3, A4, and A5;

[0065] (6) The test data results are shown in Table 1.

[0066] Table 1

[0067]

[0068] As can be seen from Table 1, compared with the blank sample, the 80μm and 200μm sieve residues of samples A3, A4, and A5 prepared by adding the cement raw material additive in Example 1 were significantly reduced, with an average reduction of 18.09% and 18.28% respectively; compared with the CD type additive, the 80μm and 200μm sieve residues of the three samples prepared by adding the cement raw material additive in Example 1 were reduced, with an average reduction of 8.94% and 11.48% respectively; compared with HX-SZY-I, the 80μm and 200μm sieve residues of the cement raw material additive prepared by adding the cement raw material additive in Example 1 were reduced, with an average reduction of 7.39% and 9.47% respectively; the content of particles ﹤3μm in the three samples prepared by adding the cement raw material additive in Example 1 was higher than that of the blank and the commercially available similar CD type and HX-SZY-I type additives. The products are significantly reduced, with an average reduction of 23.45%, 5.38% and 5.81% respectively; the average calorific value of the three samples of cement raw material additive prepared by adding Example 1 is 944Kcal / kg and 603Kcal / kg higher than the similar CD type and HX-SZY-I type additive products on the market; the calorific value of the three samples of cement raw material additive prepared by adding Example 1 is better than the similar CD type and HX-SZY-I type cement raw material additive products, and the average f-CaO content is 12.25% and 9.10% lower than the similar CD type and HX-SZY-I type additive products. In view of the above experimental data results, it is proved that a synthetic cement raw material additive mentioned in the invention can significantly improve the grinding efficiency of cement raw material and improve the calorific value of cement raw material, and is better than similar products in the same industry.

[0069] Performance Test 2 Industrial production situation of Φ1800×1700 roller mill cement raw meal final grinding system of Jiangxi DA Cement Company of WNQ Group in China.

[0070] (1) The cement raw material ratio is: limestone: high silicon: ash: shale = 85.3:6.2:2.6:5.9.

[0071] (2) synthesizing cement raw material additives according to the process steps of Example 1 above;

[0072] (3) The above-mentioned cement raw material mix is ​​mixed in proportion and then placed in a roller mill final grinding system for continuous grinding for 72 hours, and the average mixed sample is taken as a blank sample, with the sample number being B0;

[0073] (4) adding commercially available CD type and HX-SZY-I type cement raw material additives and the synthetic cement raw material additive of Example 1 of the present invention, and grinding them continuously for 72 hours respectively, and the operation is the same as (3), wherein the CD type is mixed at a ratio of 0.15%, the HX-SZY-I type is mixed at a ratio of 0.12%, and the synthetic cement raw material additive of Example 1 of the present invention is mixed at a ratio of 0.09%, and the test samples are numbered B1, B2, and B3 respectively;

[0074] (5) The experimental data of raw meal fineness, mill output, raw meal grinding power consumption, corresponding cement clinker quality and coal consumption during the entire industrial test are summarized in Tables 2 and 3.

[0075] Table 2

[0076]

[0077] Table 3

[0078]

[0079]

[0080] From Tables 2 and 3, we can conclude that:

[0081] Compared with the blank sample, at the same operating time, the 60μm and 200μm sieve residues of the additive prepared in Example 1 were reduced by 6.25% and 8% respectively, the mill output was increased by 20t / h, and the unit power consumption was reduced by 0.53kWh / t; compared with CD type and HX-SZY-I type cement raw material additives, at the same operating time, the 60μm and 200μm sieve residues of the additive prepared in Example 1 were basically consistent, the mill output was increased by 5t / h, and the unit power consumption was reduced by 0.12kWh / t and 0.14kWh / t respectively; compared with the blank sample, at the same operating time, the raw material prepared in Example 1 was added to the kiln for calcination, the clinker output was increased by 7.68t / h, the clinker standard coal was reduced by 3.64kg / t, and the qualified rate of f-CaO of the clinker out of the kiln was kept high, and the 3-day and 28-day The compressive strength at 3 days and 28 days was increased by 0.8MPa and 1.0MPa respectively; compared with CD type cement raw meal additive, with the same operation time, the raw meal prepared by Example 1 was added to the kiln for calcination, the clinker output was increased by 5.57t / h, the clinker standard coal was reduced by 1.01kg / t, and the qualified rate of f-CaO of the clinker out of the kiln was kept high, and the compressive strength at 3 days and 28 days was increased by 0.6MPa and 0.6MPa respectively; compared with HX-SZY-I type cement raw meal additive, with the same operation time, the raw meal prepared by Example 1 was added to the kiln for calcination, the clinker output was increased by 4.3t / h, the clinker standard coal was reduced by 0.94kg / t, and the qualified rate of f-CaO of the clinker out of the kiln was kept high, and the compressive strength at 3 days and 28 days was increased by 0.5MPa and 0.4MPa respectively. In view of the above industrial test data results, it is proved that the synthetic cement raw material additive mentioned in the invention can significantly improve the grinding efficiency of cement raw material and improve the burnability of cement raw material, and is superior to similar products in the same industry.

[0082] Performance test 3 is the industrial production situation of HRM4800 vertical mill cement raw material grinding system of Shaanxi QX Cement Company of HL Group.

[0083] (1) The raw material ratio is limestone: clay: sandstone: iron powder: coal gangue = 90.1:1.5:3.4:4.0:1.0.

[0084] (2) After the raw cement mix ratio is measured and mixed, it is put into the vertical mill raw grinding system for continuous grinding for 72 hours, and the average mixed sample is taken as the blank sample, and the sample number is C0;

[0085] (3) Add commercially available CD type and HX-SZY-I type cement raw material additives, and the cement raw material additive prepared in Example 1, and grind them continuously for 72 hours respectively. The operation is the same as (3), wherein the CD type is mixed at a ratio of 0.15%, the HX-SZY-I type is mixed at a ratio of 0.12%, and the cement raw material additive in Example 1 is mixed at a ratio of 0.09%. The test samples are numbered C1, C2, and C3 respectively;

[0086] (4) The experimental data of raw material fineness, mill output, raw material grinding power consumption, corresponding cement clinker quality and coal consumption during the entire industrial test are summarized in Tables 4 and 5.

[0087] Table 4

[0088]

[0089] Table 5

[0090]

[0091]

[0092] Note: The coal received has a basic calorific value of 5025Kcal / kg, external moisture of 10.1%, internal moisture of 2.92%, ash of 24.04%, and volatile matter of 27.45%.

[0093] From Tables 4 and 5, we can conclude that:

[0094] (1) Compared with the blank sample, at the same operating time, the 80μm and 200μm sieve residues of the cement raw material additive prepared by adding Example 1 were reduced by 4.54% and 7.14%, respectively, the mill output increased by 24.2t / h, and the unit power consumption decreased by 0.46kWh / t; compared with CD type and HX-SZY-I type cement raw material additives, at the same operating time, the 80μm and 200μm sieve residues of the cement raw material additive prepared by adding Example 1 were basically the same, the mill output increased by 9.7t / h and 4.9t / h, respectively, and the unit power consumption decreased by 0.29kWh / t and 0.16kWh / t, respectively; compared with the blank sample, at the same operating time, the raw material prepared by adding Example 1 was calcined in the kiln, the clinker output increased by 8.63t / h, the clinker standard coal decreased by 4.26kg / t, and the clinker f-Ca out of the kiln was calcined. O qualified rate remains the same, and its compressive strength at the age of 3 days and 28 days is increased by 1.2MPa; compared with CD type cement raw meal additive, with the same operating time, the raw meal prepared by Example 1 is added into the kiln for calcination, the clinker output is increased by 6.62t / h, the clinker standard coal is reduced by 1.76kg / t, and the f-CaO qualified rate of the clinker out of the kiln is kept consistent, and its compressive strength at the age of 3 days and 28 days is increased by 1MPa; compared with HX-SZY-I type cement raw meal additive, with the same operating time, the raw meal prepared by Example 1 is added into the kiln for calcination, the clinker output is increased by 6.88t / h, the clinker standard coal is reduced by 1.61kg / t, and the f-CaO qualified rate of the clinker out of the kiln is kept consistent, and its compressive strength at the age of 3 days and 28 days is increased by 1.2MPa and 1.1MPa respectively. In view of the above industrial test data results, it is proved that the synthetic cement raw meal additive mentioned in the invention can significantly improve the grinding efficiency of cement raw meal and improve the burnability of cement raw meal in the vertical mill and roller mill raw meal final grinding system, and is superior to similar products in the same industry.

Claims

1. A synthetic cement raw material additive, characterized in that: The raw materials include, by mass percentage: 15-40% of synthetic organic acid salt, 12-28% of synthetic organic ester, 2-9% of high-efficiency diffusant, and the balance of deionized water; The high-efficiency diffuser is a composition of nano light diffuser JSY-168 and sodium dodecyl sulfate, and the mass ratio of the composition of nano light diffuser JSY-168 and sodium dodecyl sulfate is 1:

2.

2. A method for preparing a synthetic cement raw material additive as claimed in claim 1, characterized in that: The following steps are involved: (1) preparing a synthetic organic acid salt in a reactor; (2) preparing a synthetic organic ester in a reactor; (3) adding the synthetic organic acid salt, the synthetic organic ester, the high-efficiency dispersant and deionized water into the reactor, stirring at a speed of 50 to 80 r / min for 10 to 30 min, then controlling the temperature at 60 to 80° C., stirring at a speed of 80 to 120 r / min, reacting for 30 to 50 min, and cooling to obtain the product.

3. The method for preparing a synthetic cement raw material additive according to claim 2, characterized in that: The specific method of step (1) is: add 20-40% alkaline inorganic solution and organic acid into a reaction kettle, control the temperature to 60-80°C, stir and react at a speed of 45-55 r / min for 30-50 minutes, and obtain the synthesized organic acid salt.

4. The method for preparing a synthetic cement raw material additive according to claim 3, characterized in that: The organic acid is at least one of formic acid, acetic acid, propionic acid, butyric acid, phthalic acid, adipic acid, benzoic acid, salicylic acid, caffeic acid, citric acid, oxalic acid, tartaric acid, and succinic acid.

5. The use of the synthetic cement raw material additive according to claim 1, characterized in that: The synthetic cement raw material additive is added at the raw material mixing warehouse before the new dry process cement raw material enters the mill, and is accurately metered and added according to the designed mixing amount using a special additive metering pump.

6. The use of the synthetic cement raw material additive according to claim 5, characterized in that: The blending mass proportion of the synthetic cement raw material additive is 0.7‰ to 1.1‰.

Citation Information

Patent Citations

  • Cement raw material additive and preparation method thereof

    CN113800796A

  • A cement raw material grinding aid, its preparation method and application

    CN114477844B

  • Cement raw material grinding aid as well as preparation method and application thereof

    CN114477844A

  • High-strength cement clinker and production process thereof

    CN115057635A