A method for improving the anti-drying cracking property of alkali slag by using a hot-soluble modified activator
By reacting high concentration of sodium hydroxide and sodium fluorosilicate under boiling conditions, the precipitation and crystallization of water glass is accelerated, and a modified exciter is prepared, which solves the problem of alkali slag being prone to dryness and cracking, significantly improves its resistance to dryness and cracking and reduces The occurrence of dry cracks.
Patent Information
- Application Number
- CN202310214989.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-08
AI Technical Summary
Alkaline slag is prone to dryness and cracking in natural or dry environments. The prior art is difficult to effectively improve its resistance to dryness and cracking, and the solubility of sodium fluorosilicate is poor at room temperature, so it cannot effectively exert its curing effect.
By reacting high concentration of sodium hydroxide and sodium fluosilicate under boiling conditions, the dissolution of sodium fluosilicate active ions is promoted and chemical reaction with liquid water glass is carried out to accelerate the precipitation and crystal hardening of water glass, and a modification excitant is prepared. To enhance the condensation and hardening process of alkali slag.
It significantly improves the anti-cracking properties of alkali slag, avoids the dehydration of water glass reaction products in a natural dry environment, and significantly reduces the occurrence of macroscopic drying and cracking. The prepared crack-resistant alkali slag concrete has not been dried after a long period of natural air drying. Significant dry cracks were seen.
Smart Images

Figure CN116283092B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building material production, and in particular relates to a method for improving the dry crack resistance of alkali slag by using a hot-soluble modified activator. Background Art
[0002] As a new type of inorganic cementitious material, alkali-activated slag not only does not require the high-energy consumption production process of silicate cement, but also has better early-strength and high-strength mechanical properties than silicate cement. Although these advantages give alkali-activated slag a very broad application prospect, an obvious disadvantage of alkali-activated slag is its poor volume stability. When it is in a natural or dry environment, it has a greater water loss characteristic than silicate cement. This leads to a series of adverse consequences, among which macroscopic cracking is a more serious destructive phenomenon, which seriously restricts the application of alkali-activated slag in actual engineering.
[0003] At present, it is generally recognized that liquid water glass with low modulus (1.0-2.0) is the best activator for alkali slag. However, many studies have also shown that alkali-activated slag prepared with liquid water glass has the most obvious dry cracking characteristics, and the more liquid water glass is added, the more severe the cracking. This is because the alkali slag frozen body activated by liquid water glass is composed of three parts: slag particles wrapped in gel, water glass cores overlapped by polymerization reaction products, and hardened water glass true solution. When the alkali slag solidifies, the slow hardening characteristic of liquid water glass causes it to exist in the alkali slag frozen body in an incompletely crystallized form. When in a natural dry environment, the reaction products involving water glass components in the alkali slag frozen body will easily dehydrate, causing macroscopic cracking.
[0004] In order to solve the problem of alkali slag being easy to lose water and crack, the current engineering practice generally adopts methods such as adding expansion agents, shrinkage reducing agents and mineral admixtures to alkali slag. However, these methods do not fundamentally change the easy water loss characteristics of alkali slag frozen bodies, and there is also the problem of poor compatibility. Therefore, it is difficult to fundamentally improve the anti-cracking property of alkali slag with existing means.
[0005] Sodium fluorosilicate is a curing agent for water glass. Its solution can react chemically with liquid water glass, accelerating the precipitation of liquid water glass silica gel and the dehydration, crystallization and hardening of the true solution. However, the solubility of sodium fluorosilicate at room temperature is extremely poor. If it is directly added to water glass, it will not dissolve and precipitate and will not play any role. In the process of preparing the alkaline activator, a certain amount of sodium hydroxide needs to be added to the water glass to lower the modulus, and the dissolution of high concentration of sodium hydroxide will release a lot of heat, which just helps the dissolution of sodium fluorosilicate. This provides a potential application path for the modification of water glass activator by sodium fluorosilicate.
[0006] Chinese patent CN202010282291.3 discloses an in-situ activated geopolymer plugging agent, wherein a synergistic composite activator of sodium hydroxide, water glass and sodium fluorosilicate is first embedded in chitosan particles; then, the geopolymer raw materials (metakaolin, red mud and volcanic ash powder) are pre-meshed by a high-temperature and high-pressure kneading machine, and then, nanofibers and microfibers are mixed in, and on this basis, the pre-embedded activator is added and further meshed, thereby forming a geological plugging agent with in-situ activation characteristics. After entering the leaking layer, the chitosan wall softens, squeezes, and breaks, releasing the composite activator, reacting with the raw materials to quickly generate geopolymers. At the same time, through the stretching effect of nano-micron fibers, the strength and toughness of the polymer plugging layer are improved, thereby playing a role in rapid plugging and improving the pressure bearing capacity of the well wall. The composite activator proposed in the prior art CN202010282291.3 is prepared by a long-term high-temperature stirring reaction in a high-pressure autoclave of a high-pressure reactor, and its economic benefits are low compared to the modified activator of this application. Secondly, the sodium fluorosilicate in the composite activator is a modification of powdered water glass, and this application is aimed at liquid water glass. The existing alkali slag basically uses liquid water glass as a raw material, and there is a large gap in the reaction activity of powdered water glass and liquid water glass. Finally, CN202010282291.3 does not emphasize that its composite activator has the effect of improving the anti-cracking property of alkali slag, but emphasizes the effect of improving its strength and toughness under the action of fibers. Summary of the invention
[0007] Technical issues solved:
[0008] In view of the shortcomings of the prior art, the present application provides a method for using a hot-soluble modified activator to improve the anti-cracking property of alkali slag, which solves the current problems such as poor volume stability of alkali slag, more severe macroscopic cracking with increasing water glass content, poor compatibility, and extremely poor solubility of sodium fluorosilicate at room temperature.
[0009] Technical solution:
[0010] To achieve the above objectives, this application is implemented through the following technical solutions:
[0011] A method for improving the dry cracking resistance of alkali slag by using a hot-soluble modified activator, comprising the following steps:
[0012] Step 1: Mix sodium hydroxide and water in a ratio of 1:1 to 1.5 to form a hot strong alkaline solution;
[0013] Step 2: Add sodium fluorosilicate to the heated strong alkaline solution while stirring to promote the dissolution of active ions in the sodium fluorosilicate.
[0014] Until the dissolved liquid boils;
[0015] Step 3: immediately after boiling, add liquid water glass to the solution, then add water and mix and stir to obtain a modified activator;
[0016] Step 4: Put the modified activator, slag, sand and gravel into the concrete mixer and stir for 135 to 225 seconds;
[0017] Step 5: Finally, pour into the mold, remove the mold after the slurry solidifies and hardens, and then place it in a standard concrete curing room for 7 to 30 days.
[0018] Furthermore, in the first step, sodium hydroxide and water are mixed in a ratio of 1:1.2 to form a heated strong alkaline solution.
[0019] Furthermore, the mass of the sodium fluorosilicate accounts for 8% to 15% of the mass of the water glass.
[0020] Furthermore, the solid components in the liquid water glass are SiO2 and Na2O, and the solid content of the liquid water glass is 10-20% of the mass of the slag.
[0021] Furthermore, the mass of the sodium hydroxide is the mass required to adjust the modulus of liquid water glass having a substance amount ratio of SiO2 to Na2O of 2 to 3.5 to 1 to 1.5.
[0022] Furthermore, in the fourth step, the mass ratio of slag: sand: gravel: modified activator is 4.5:5:6:2.5.
[0023] Furthermore, the amount of water added in the third step is 25% to 35% of the mass of the slag.
[0024] Furthermore, the slag has a specific surface area of 450 m 2 / kg; the sand is river sand with a particle size of ≤4.75mm; the gravel is composed of three types of gravel with particle sizes of 19-31mm, 13-18mm and 5-12mm respectively, and the mass ratio is 9:8:6.
[0025] The principle of the present invention is as follows: the present invention proposes a method for improving the anti-drying cracking property of alkali slag by using a hot-soluble modified activator. The method adopts a freshly prepared high-concentration sodium hydroxide alkali solution to boil and dissolve sodium fluorosilicate, promotes the dissolution of active ions in the sodium fluorosilicate, and then adds water glass and water to the dissolved solution to obtain a modified alkali slag activator; the modified activator is used to mix the alkali slag slurry, which can accelerate the large-scale decomposition and precipitation of water glass SiO2 nuclei during the coagulation and hardening process of the alkali slag, and increase the crystallization degree of the water glass true solution in the alkali slag frozen body, thereby improving the easy water loss characteristic of the alkali slag caused by the water glass, and achieving the purpose of improving the anti-drying cracking property of the alkali slag from the root.
[0026] Beneficial effects:
[0027] The present application provides a method for improving the anti-drying cracking property of alkali slag by using a hot-soluble modified activator, which has the following beneficial effects:
[0028] 1. Use high-concentration sodium hydroxide lye to boil and dissolve the active ions in sodium fluorosilicate. Sodium fluorosilicate is a curing agent for water glass. Its active dissolving liquid can react chemically with water glass to accelerate the precipitation of water glass silica gel and the dehydration, crystallization and hardening of the true solution. However, the solubility of sodium fluorosilicate at room temperature is very poor. If it is directly added to water glass, it will only precipitate without any effect. In the process of preparing the alkali activator, a certain amount of sodium hydroxide needs to be added to the water glass to lower the modulus. The dissolution of high-concentration sodium hydroxide will release a lot of heat, which just helps the dissolution of sodium fluorosilicate.
[0029] 2. Our exploratory experiments have found that high-concentration sodium hydroxide lye can react with sodium fluorosilicate to produce a boiling reaction. In the early stage of the boiling phenomenon, the lye causes a large amount of active ions in sodium fluorosilicate to dissolve. At this time, adding water glass can not only avoid the complete reaction between sodium fluorosilicate and the lye to generate new substances, but also give full play to the role of active ions in sodium fluorosilicate to accelerate the solidification of water glass;
[0030] 3. The alkali slag frozen body is composed of slag particles wrapped in gel, water glass cores overlapped by polymerization reaction products, and hardened water glass true solution. The slow hardening property of water glass makes it exist in the alkali slag frozen body in the form of incomplete crystallization. When in a natural dry environment, the reaction products involving water glass components in the alkali slag frozen body will be easily dehydrated, causing the properties of the products to change and cause macroscopic cracking. The crystallization and hardening of water glass is accelerated by dissolving sodium fluorosilicate, and the macroscopic cracking induced by water glass is solved;
[0031] 4. The present invention achieves water glass activator modification by thermally dissolving sodium fluorosilicate in high-concentration alkali solution. The modified activator can accelerate the large-scale decomposition and precipitation of water glass SiO2 nuclei during the coagulation and hardening process of alkali slag, and greatly improve the crystallization degree of water glass true solution in the alkali slag frozen body, completely avoiding the dehydration of the reaction products involving water glass in the hardened alkali slag frozen body in a natural drying environment, thereby fundamentally improving the anti-cracking property of the alkali slag;
[0032] 5. Compared with the existing traditional alkali slag, the anti-cracking coefficient of the alkali slag concrete prepared by the present invention is better, and after long-term natural air drying, no obvious drying cracks are observed on the surface cement stone under a video electron microscope. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a diagram showing the cracking of the surface of the hot-soluble modified alkali-slag concrete after long-term air drying in this application.
[0034] Figure 2This is a diagram showing the cracking of the surface of traditional alkali-slag concrete after long-term air drying. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0036] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the protection scope of the present invention.
[0037] The proportion of alkali slag is any amount of sodium silicate water glass, sodium hydroxide, water and slag that can effectively polymerize the alkali slag precursor and build strength.
[0038] Embodiment 1:
[0039] A method for improving the anti-drying cracking property of alkali slag by using a hot-soluble modified activator, wherein the solid components in the liquid water glass are SiO2 and Na2O, and the solid content of the liquid water glass is 10-20% of the mass of the slag. The Na2O content of the liquid water glass is 9.65%, the SiO2 content is 25.22%, the water content is 65%, and the ratio of the modulus SiO2 of the liquid water glass to the amount of Na2O is 2-3.5. The mass of sodium hydroxide is the mass required to adjust the modulus of the liquid water glass to 1.5; the mass of sodium fluorosilicate is 12% of the mass of the liquid water glass.
[0040] The preparation process of the modified activator is as follows: sodium hydroxide and water are mixed in a ratio of 1:1.2 to form a heated strong alkaline solution; sodium fluorosilicate is added to the heated strong alkaline solution while stirring until the dissolved liquid boils; after the solution is stirred to boiling, liquid water glass is immediately added thereto, and then water is added and mixed to obtain the modified activator, wherein the amount of water added is 25% to 35% of the mass of the slag.
[0041] A method for improving the dry cracking resistance of alkali slag by using a hot-soluble modified activator is applied to the preparation process of crack-resistant alkali slag concrete, which is as follows: the modified alkali activator, slag, sand and gravel are poured into a concrete mixer according to the mass ratio of slag: sand: gravel: modified activator = 4.5:5:6:2.5 and stirred for 180 seconds. The specific surface area of the slag is 450m 2 / kg; the sand is river sand with a particle size of ≤4.75mm; the gravel is composed of three types of gravel with particle sizes of 19-31mm, 13-18mm and 5-12mm respectively, and the mass ratio is 9:8:6.
[0042] Finally, pour it into the mold, let it stand for 1 day until the slurry solidifies and hardens, then remove the mold, and then put it into a standard curing room for 28 days. The slump of the crack-resistant alkali slag concrete prepared in this embodiment is 180mm, the compressive strength is 58.8MPa, and the cracking coefficient measured according to the "Test Method for Drying Shrinkage Cracking Performance of Cement Mortar and Concrete" (GB / T29417-2012) is 0.42. The concrete was placed in a natural environment to air dry for 28 days, and observed under 50x magnification using a video electron microscope. Figure 1 As shown, there are no obvious cracks on the surface of the cement stone.
[0043] Comparative Example 1
[0044] An existing traditional alkali slag concrete, the alkali activator ratio of which is: the solid content of liquid water glass (the sum of SiO2 and N2O mass) is 17.5% of the mass of slag. The Na2O content of the liquid water glass is 9.65%, the SiO2 content is 25.22%, and the water content is 65%. The mass of sodium hydroxide is the mass required to adjust the modulus of the liquid water glass to 1.5.
[0045] The raw materials are mixed in a mass ratio of slag: sand: gravel: alkali activator = 4.5:5:6:2.4. The alkali activator, slag, sand and gravel are poured into a concrete mixer and stirred for 180 seconds. The specific surface area of the slag is 450m 2 / kg; the sand is river sand with a particle size of ≤4.75mm; the gravel is composed of three types of gravel with particle sizes of 19-31mm, 13-18mm and 5-12mm respectively, and the mass ratio is 9:8:6.
[0046] Finally, pour it into the mold, let it stand for 1 day, then remove the mold, and then put it in a standard curing room with a temperature of 20±2°C and a relative humidity of more than 95% for 28 days. The slump of the crack-resistant alkali slag concrete prepared in this embodiment is 185mm, the compressive strength is 57.5MPa, and the cracking coefficient measured according to the "Test Method for Drying Shrinkage Cracking Performance of Cement Mortar and Concrete" (GB / T29417-2012) is 0.92. The concrete was placed in a natural environment to air dry for 28 days, and observed under a video electron microscope at 50 times magnification. Figure 2 As shown, obvious drying cracks can be seen on the surface of the cement stone.
[0047] The above is a detailed description of the present invention in combination with the embodiments, but the implementation methods of the present invention are not limited to the above embodiments. Improvements, replacements, and modifications made by those skilled in the art based on the inspiration of the present invention and without departing from the core guiding ideology of the present invention should all be within the scope of protection of the present invention.
Claims
1. A method for improving the dry cracking resistance of alkali slag by using a hot-soluble modified activator, characterized in that: The steps are: Step 1: Mix sodium hydroxide and water in a ratio of 1:1~1.5 to form a hot strong alkaline solution; Step 2: Add sodium fluorosilicate to the heated strong alkaline solution while stirring to promote the dissolution of active ions in the sodium fluorosilicate until the solution boils; Step 3: immediately after boiling, liquid water glass is added to the dissolved liquid, and then water is added and mixed to obtain a modified activator; the solid components in the liquid water glass are SiO2 and Na2O, and the solid content of the liquid water glass is 10-20% of the mass of the slag; Step 4: Put the modified activator, slag, sand and gravel into a concrete mixer and stir for 135-225 seconds; the mass ratio of slag: sand: gravel: modified activator is 4.5:5:6:2.5; the specific surface area of the slag is 450 m 2 / kg; the sand is river sand with a particle size of ≤4.75 mm; the gravel is composed of three types of gravel with particle sizes of 19~31 mm, 13~18 mm and 5~12 mm, respectively, with a mass ratio of 9:8:6; Step 5: Finally, pour into the mold, remove the mold after the slurry solidifies and hardens, and then place it in a standard concrete curing room for 7 to 30 days.
2. The method for improving the dry cracking resistance of alkali slag by using a hot-soluble modified activator according to claim 1, characterized in that: In the first step, sodium hydroxide and water are mixed in a ratio of 1:1.2 to form a heated strong alkaline solution.
3. The method for improving the dry cracking resistance of alkali slag by using a hot-soluble modified activator according to claim 1, characterized in that: The mass of the sodium fluorosilicate accounts for 8% to 15% of the mass of the water glass.
4. The method for improving the dry cracking resistance of alkali slag by using a hot-soluble modified activator according to claim 1, characterized in that: The mass of the sodium hydroxide is the mass required to adjust the modulus of liquid water glass having a ratio of the amount of substance of SiO2 to Na2O of 2-3.5 to 1-1.
5.
5. The method for improving the dry cracking resistance of alkali slag by using a hot-soluble modified activator according to claim 1, characterized in that: The amount of water added in the third step is 25% to 35% of the slag mass.