High-performance low-shrinkage concrete containing lightweight aggregate and preparation method thereof
By adding ceramics and shale ceramic sand to light concrete and using defoaming agent, the problems of light aggregate floating and high temperature burst are solved, and the high strength, low shrinkage and good homogeneity of concrete are achieved, which improves the Engineering quality and structural safety.
Patent Information
- Application Number
- CN202410902574.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-07
AI Technical Summary
Traditional lightweight concrete is easy to float when ensuring fluidity, which makes it difficult to ensure homogeneity, affects the quality of the project, and is prone to burst under high temperature conditions, reducing structural safety.
By adding ceratops and shale clay sand and using defoaming agent, the concrete mix ratio is optimized, the clay and clay sand is pre-wet, and the raw materials such as cement, fly ash, silica fume, and gravel are reasonably matched, and polycarboxylate is used. Acid water reducer and modified silicone defoaming agent to control the apparent density and structural compactness of concrete.
It effectively reduces the apparent density of concrete, ensures uniform distribution of lightweight aggregates, improves the strength, bending and crack resistance of concrete, inhibits the generation of pores and cracks, and significantly improves the durability and safety of concrete.
Smart Images

Figure CN119019131A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, in particular to a high-performance low-shrinkage concrete containing lightweight aggregate and a preparation method and application thereof. Background Art
[0002] With the development and construction of the country, the demand for large buildings and long-span bridges is becoming stronger and stronger, and the requirements for lightweight, high-strength, green, and durable civil engineering materials are also getting higher and higher. As one of the most common materials in bridge engineering, the density of traditional concrete is high, which directly leads to a large self-weight of the structure, limiting the development of the span of concrete bridges. The lightweight of concrete can effectively reduce the self-weight ratio of bridges and increase the effective load ratio of bridges. For the external curtain wall structure of large buildings, the pursuit of high-temperature resistant, lightweight and high-strength concrete structures has become an inevitable trend.
[0003] High-performance low-shrinkage concrete containing lightweight aggregate is a high-performance concrete with a strength exceeding 60MPa designed based on the maximum packing density theory. HSLC (high-strength lightweight concrete) has high strength and lightweight properties. In the construction field, it can reduce the deadweight of the structure, thereby reducing the amount of materials used and reducing carbon emissions. HSLC highlights unique advantages in the fields of bridge engineering, underground structures and high-rise buildings. In order to further develop the application scenarios of HSLC, it is of great significance to develop a HSLC that can meet the structural performance requirements, reduce the deadweight of the structure, and improve the structural safety.
[0004] However, it was also found during use that while traditional lightweight concrete ensures fluidity, the lightweight aggregate floats severely, and its own homogeneity is difficult to ensure, which seriously affects the quality of the project. The main reason is that the lightweight aggregate used in lightweight concrete has a small specific gravity and is easy to float in the concrete. How to effectively control the floating of lightweight aggregate in lightweight concrete is an important prerequisite for ensuring its engineering performance; in addition, due to the dense internal structure of HSLC and few defects, it is very easy to burst under high temperature conditions, causing great damage to the structure and the surrounding environment, and reducing safety under high temperature conditions.
[0005] Starting from the use and selection of raw materials, high-quality and high-strength lightweight aggregates and composite polycarboxylic acid admixtures that adjust working performance are selected; and the mix ratio of lightweight and high-strength concrete is designed and optimized based on the theoretical "strength matching principle" and "interface enhancement theory"; the prepared lightweight and high-strength concrete has good workability, homogeneity, durability and crack resistance, and is used in supporting projects. Summary of the invention
[0006] The present invention proposes a lightweight, high-temperature-resistant, high-performance, low-shrinkage concrete, which not only reduces the concrete bulk density (can be reduced to 1700kg / m3 ) At the same time, it does not cause major changes in performance; and it also solves the problem of easy floating of expanded clay and sand and explosion of concrete.
[0007] The present invention provides a high-performance low-shrinkage concrete with lightweight aggregate, wherein the concrete is mixed with the following raw materials in percentage by weight:
[0008] Cement 19%-21%, first-grade fly ash 4%-6%, silica fume 12%-15%, water 5%-8%, crushed stone 28%-32%, expanded clay 5%-10%, river sand 15%-20%, 900-grade shale expanded clay 5%-10%, water reducer 5%, and defoaming agent 0.01%.
[0009] Preferably, the cement is 42.5 ordinary Portland cement.
[0010] Preferably, the fly ash is primary fly ash.
[0011] Preferably, the specific surface area of the silica fume is ≥19000m 2 / kg, of which SiO2 content is ≥90%.
[0012] Preferably, the crushed stone is basalt crushed stone with a particle size of 5-10 mm and a continuous gradation.
[0013] Preferably, the ceramsite is fly ash ceramsite with a bulk density of 1600 kg / m 3 ~1800kg / m 3 It is composed of 5-12mm size, with a cylinder pressure strength of 13.1MPA, 1h water absorption rate of 4.8%, softening coefficient of 0.9, and the sum of breakage rate and wear rate of 3.1%.
[0014] Preferably, the river sand is medium sand with a fineness modulus of 2.3-2.6.
[0015] Preferably, the shale ceramic sand is grade 900 and has a bulk density of 900 kg / m 3 ~1400kg / m 3 It is composed of large, medium and small sizes of 0.5-0.35mm, 0.35-0.25mm, and 0.160-0.25, and the weight ratio of large, medium and small sizes of shale ceramic sand is 60-65:20-25:10-20. The cylinder pressure strength is greater than 5MPA, and the chemical composition is mainly silicon dioxide, aluminum oxide, iron oxide, and calcium oxide.
[0016] Preferably, the water reducer is a polycarboxylate water reducer.
[0017] Preferably, the main component of the defoaming agent is modified silicone.
[0018] The present invention also provides a method for preparing the lightweight aggregate high-performance low-shrinkage concrete, which comprises the following steps:
[0019] S1, pre-wetting the ceramsite to obtain pre-wet ceramsite;
[0020] S2, stirring water and the admixture to obtain a first mixture;
[0021] S3, adding the cement, primary fly ash, silica fume and fine aggregate into a forced mixer and dry mixing for 1-2 minutes to uniformly mix the cementitious material and the fine aggregate to obtain a second mixture;
[0022] S4, uniformly mix the first mixture and the second mixture, add coarse aggregate into the mixing equipment and stir for 1-2 minutes, so that the coarse aggregate can be well wrapped by the mortar, and the concrete can be formed;
[0023] S5, forming the concrete in a mold and performing moisture-keeping curing.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The lightweight high-performance concrete disclosed by the present invention, on the one hand, greatly reduces the apparent density of concrete by adding lightweight components such as ceramsite and ceramic sand, thereby achieving the purpose of lightweight high-performance concrete; at the same time, a reasonable proportion is used to make the lightweight aggregate evenly distributed in the concrete, thereby making the stress distribution even, so that the strength, bending resistance and impact resistance of the concrete are significantly improved; adding a defoaming agent to the base concrete can effectively inhibit the generation of concrete pores and macro cracks, and can improve the crack resistance, tensile resistance, bending resistance and impact resistance of the concrete; a series of lightweight concrete with strength grades of LC60-LC80 and densities of 1700-2150kg / m° can be prepared.
[0026] The lightweight high-performance concrete provided by the present invention is based on the most compact packing density theory in the HSLC preparation technology, and uses pottery sand to replace the river sand in the traditional concrete, thereby solving the problem of high apparent density of the traditional concrete. The interior of the pottery sand is honeycomb-shaped and has low thermal conductivity. The apparent density of the concrete with traditional river sand as aggregate is 2400kg / m~2600kg / m. The apparent density of the UHPC using pottery sand as aggregate in the present invention can be reduced to 1600kg / m~2000kg / m, which greatly reduces the apparent density of the concrete.
[0027] The main components of the defoamer in the present invention include polyether and modified silicone, which can destroy the foam film and make the foam disappear quickly, thereby making the concrete surface more compact, effectively inhibiting the bubbles generated in the concrete, inhibiting the microcracks caused by factors such as plastic shrinkage, drying shrinkage, and temperature changes, and greatly improving the anti-cracking performance and anti-abrasion performance of the concrete.
[0028] The lightweight high-performance concrete provided by the present invention is advantageous for use in the transportation, hoisting and splicing of prefabricated structures, and is advantageous for promoting the development of prefabricated high-performance concrete and accelerating the progress of projects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0030] Figure 1 It is a schematic cross-sectional view of the high performance low shrinkage concrete after forming in the present invention. DETAILED DESCRIPTION
[0031] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.
[0032] In the description of the present invention, it should be noted that the terms "inside", "outside", "up", "down", "horizontal", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the present invention.
[0033] Example 1, a high-performance low-shrinkage concrete with lightweight aggregate is prepared by mixing the following raw materials in parts by weight: 41 parts of cement, 11 parts of first-grade fly ash, 2.75 parts of silica fume, 14.3 parts of water, 60 parts of crushed stone, 17.5 parts of ceramsite, 36.2 parts of river sand, 14 parts of 900-grade shale ceramsite, 2.75 parts of water reducer, and 0.5 parts of defoamer;
[0034] In this embodiment, the shale ceramic sand is grade 900 and has a bulk density of 1230 kg / m 3 , consisting of large, medium and small sizes of 0.5-0.35mm, 0.35-0.25mm, and 0.160-0.25mm, and the weight ratio of large, medium and small sizes of pottery sand is 60:25:20.
[0035] In this embodiment, the fly ash is primary fly ash.
[0036] In this embodiment, the specific surface area of the silica fume is ≥19000m 2 / kg, of which SiO2 content is ≥90%.
[0037] In this embodiment, the crushed stone is basalt crushed stone with a particle size of 5-10 mm and a continuous gradation.
[0038] In this embodiment, the ceramsite is fly ash ceramsite with a bulk density of 1600 kg / m 3 ~1800kg / m 3 It is composed of 5-12mm size, with a cylinder pressure strength of 13.1MPA, 1h water absorption rate of 4.8%, softening coefficient of 0.9, and the sum of breakage rate and wear rate of 3.1%.
[0039] In this embodiment, the river sand is medium sand with a fineness modulus of 2.3-2.6.
[0040] In this embodiment, the water reducing agent is specifically a polycarboxylic acid high performance water reducing agent;
[0041] In this embodiment, the defoaming agent is a silicone liquid defoaming agent.
[0042] The preparation method of the high performance low shrinkage concrete with lightweight aggregate in this embodiment is as follows:
[0043] First, the ceramsite is placed in water for pre-wetting for 72 hours to obtain pre-wet ceramsite.
[0044] Then, the water and the additive are stirred evenly to obtain a first mixture;
[0045] Subsequently, the silicate cement, primary fly ash, silica fume and fine aggregate are added into a forced mixer and dry-mixed for 1-2 minutes to uniformly mix the cementitious material and the fine aggregate to obtain a second mixture;
[0046] Finally, the first mixture and the second mixture are uniformly mixed, the mixer speed is adjusted to 200r / min, and the uniform low-speed mixing is continued for 1-2 minutes to form the concrete;
[0047] Embodiment 2 is different from the above-mentioned embodiment 1 in that:
[0048] A high-performance low-shrinkage concrete with lightweight aggregate in this embodiment is prepared by mixing the following raw materials in parts by weight: 41 parts of cement, 11 parts of first-grade fly ash, 2.75 parts of silica fume, 14.3 parts of water, 50 parts of crushed stone, 32.5 parts of ceramsite, 36.2 parts of river sand, 14 parts of 900-grade shale ceramsite, 2.75 parts of water reducer, and 0.5 parts of defoamer;
[0049] The shale ceramic sand is grade 900 and has a bulk density of 1230 kg / m 3 , consisting of large, medium and small sizes of 0.5-0.35mm, 0.35-0.25mm, and 0.160-0.25mm, and the weight ratio of large, medium and small sizes of pottery sand is 60:25:20.
[0050] The preparation method of the high performance low shrinkage concrete with lightweight aggregate in this embodiment is as follows:
[0051] Pre-wet the expanded clay in water for 72 hours.
[0052] Then, the water and the additive are stirred evenly to obtain a first mixture;
[0053] Pre-wet the clay sand in water for 72 hours.
[0054] Then, the water and the additive are stirred evenly to obtain a first mixture;
[0055] Add the silicate cement, primary fly ash, silica fume and fine aggregate into a forced mixer and dry mix for 1-2 minutes to evenly mix the cementitious material and the fine aggregate to obtain a second mixture;
[0056] The first mixture is uniformly mixed with the second mixture, the mixer speed is adjusted to 200r / min, and the mixture is uniformly stirred at a low speed for 1-2 minutes to form the concrete.
[0057] Embodiment 3 is different from the above-mentioned embodiment 1 in that:
[0058] A high-performance low-shrinkage concrete with lightweight aggregate in this embodiment is prepared by mixing the following raw materials in parts by weight: 41 parts of cement, 11 parts of first-grade fly ash, 2.75 parts of silica fume, 14.3 parts of water, 40 parts of crushed stone, 39.1 parts of ceramsite, 36.2 parts of river sand, 14 parts of 900-grade shale ceramsite, 2.75 parts of water reducer, and 0.5 parts of defoamer;
[0059] The shale ceramic sand is grade 900 and has a bulk density of 1230 kg / m 3 , consisting of large, medium and small sizes of 0.5-0.35mm, 0.35-0.25mm, and 0.160-0.25mm, and the weight ratio of large, medium and small sizes of pottery sand is 60:25:20.
[0060] The preparation method of the high performance low shrinkage concrete with lightweight aggregate in this embodiment is as follows:
[0061] Pre-wet the expanded clay in water for 72 hours.
[0062] Then, the water and the additive are stirred evenly to obtain a first mixture;
[0063] Add the silicate cement, primary fly ash, silica fume and fine aggregate into a forced mixer and dry mix for 1-2 minutes to evenly mix the cementitious material and the fine aggregate to obtain a second mixture;
[0064] The first mixture is uniformly mixed with the second mixture, the mixer speed is adjusted to 200r / min, and the mixture is uniformly stirred at a low speed for 1-2 minutes to form the concrete.
[0065] Embodiment 4 is different from the above-mentioned embodiment 1 in that:
[0066] A high-performance low-shrinkage concrete with lightweight aggregate in this embodiment is prepared by mixing the following raw materials in parts by weight: 41 parts of cement, 11 parts of first-grade fly ash, 2.75 parts of silica fume, 14.3 parts of water, 60 parts of crushed stone, 17.5 parts of ceramsite, 28 parts of 900-grade shale sand, 2.75 parts of water reducer, and 0.5 parts of defoamer;
[0067] The shale ceramic sand is grade 900 and has a bulk density of 1230 kg / m 3 , consisting of large, medium and small sizes of 0.5-0.35mm, 0.35-0.25mm, and 0.160-0.25mm, and the weight ratio of large, medium and small sizes of pottery sand is 60:25:20.
[0068] The preparation method of the high performance low shrinkage concrete with lightweight aggregate in this embodiment is as follows:
[0069] Pre-wet the expanded clay in water for 72 hours.
[0070] Then, the water and the additive are stirred evenly to obtain a first mixture;
[0071] Add the silicate cement, primary fly ash, silica fume and fine aggregate into a forced mixer and dry mix for 1-2 minutes to evenly mix the cementitious material and the fine aggregate to obtain a second mixture;
[0072] The first mixture and the second mixture are uniformly mixed, the mixer speed is adjusted to 200r / min, and the mixing is continued uniformly at a low speed for 1-2 minutes to form the concrete;
[0073] Embodiment 5 is different from the above-mentioned embodiment 1 in that:
[0074] A high-performance low-shrinkage concrete with lightweight aggregate in this embodiment is prepared by mixing the following raw materials in parts by weight: 41 parts of cement, 11 parts of first-grade fly ash, 2.75 parts of silica fume, 14.3 parts of water, 50 parts of crushed stone, 32.5 parts of ceramsite, 28 parts of 900-grade shale sand, 2.75 parts of water reducer, and 0.5 parts of defoamer;
[0075] The shale ceramic sand is grade 900 and has a bulk density of 1230 kg / m 3 , consisting of large, medium and small sizes of 0.5-0.35mm, 0.35-0.25mm, and 0.160-0.25mm, and the weight ratio of large, medium and small sizes of pottery sand is 60:25:20.
[0076] The preparation method of the high performance low shrinkage concrete with lightweight aggregate in this embodiment is as follows:
[0077] Pre-wet the expanded clay in water for 72 hours.
[0078] Then, the water and the additive are stirred evenly to obtain a first mixture;
[0079] Add the silicate cement, primary fly ash, silica fume and fine aggregate into a forced mixer and dry mix for 1-2 minutes to evenly mix the cementitious material and the fine aggregate to obtain a second mixture;
[0080] The first mixture is uniformly mixed with the second mixture, the mixer speed is adjusted to 200r / min, and the mixture is uniformly stirred at a low speed for 1-2 minutes to form the concrete.
[0081] 1. Performance Effect
[0082] The ultra-high performance concrete prepared in the above Examples 1-5 was tested for slump, expansion, mechanical properties, and drying shrinkage. The test standards and methods are as follows:
[0083] (1) Slump test standard: GB / T50080-2016;
[0084] (2) Compressive strength and flexural strength test standards: Refer to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete" to make standard test blocks of 10cm×10cm×10cm, and test their flexural strength and compressive strength after 7d and 28d of curing.
[0085] (3) Crack resistance test: Refer to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete" to make standard test blocks. Record the number of cracks on the concrete surface after 28 days of curing at an ambient temperature of 42±2℃ to obtain the number of cracks per unit area.
[0086] (4) Shrinkage performance test: Make standard test blocks with reference to GB / T50081-2019 "Standard test methods for physical and mechanical properties of concrete", cure them in an outdoor environment at 42±2℃, and then record the 28d shrinkage rate data with reference to GB / T50082-2009 "Standard test methods for long-term performance and durability of ordinary concrete".
[0087] The results are as follows:
[0088]
[0089] From the above results, it can be seen that the ultra-high performance concrete prepared according to the present invention has higher mechanical properties, 7d flexural strength of 5-7MPa, 28d flexural strength of 7-9MPa, 7d compressive strength of 44-55MPa, 28d compressive strength of 64-71MPa, no cracks, and shrinkage rate of 0.10-0.25‰; it can be seen that the concrete of the present invention has a low shrinkage effect while also having higher strength, good durability and bearing capacity, among which Example 3 has the best effect.
[0090] A comparative example is set for comparison with the above optimal strength embodiment 5, as follows:
[0091] Comparative Example 1: The difference between this comparative example and Example 5 is that the high-performance low-shrinkage concrete with lightweight aggregate includes the following raw materials in parts by weight: 44 parts of cement, 11 parts of first-grade fly ash, 0 parts of silica fume, 14.3 parts of water, 50 parts of crushed stone, 32.5 parts of ceramsite, 28 parts of 900-grade shale sand, 2.75 parts of water reducer, and 0.5 parts of defoamer;
[0092] Comparative Example 2: The difference between this comparative example and Example 3 is that the ceramic sand is not pre-wetted.
[0093] Comparative Example 3: The difference between this comparative example and Example 3 is that no defoaming agent is added to the raw materials of the low shrinkage and cracking-resistant ultra-performance concrete;
[0094] Specifically, the raw materials include the following parts by weight: 41 parts of cement, 11 parts of first-grade fly ash, 2.75 parts of silica fume, 14.3 parts of water, 50 parts of crushed stone, 32.5 parts of ceramsite, 28 parts of 900-grade shale sand, and 2.75 parts of water reducer;
[0095]
[0096] It can be seen from the above results that, compared with Example 1, the concrete raw materials of the present invention are reasonably selected, scientifically proportioned, and their performance is synergistically exerted, with low shrinkage, strong mechanical properties, and not easy to break; compared with Example 1, adding an appropriate amount of silica fume to the concrete can fill the tiny pores and fine cracks inside the concrete, and improve the compactness and durability of the concrete. In addition, the active silica in the silica fume reacts with water to form calcium silicate cementitious materials, which can enhance the strength and hardness of the concrete; compared with Example 2, Example 5 pre-wets the ceramsite in advance, and the wet ceramsite will supplement water for cement hydration, so that the cement slurry is hydrated more thoroughly and the autogenous shrinkage is reduced.
[0097] Compared with Comparative Example 3, in Example 5, the addition of defoaming agent will cause the wet expanded clay to supplement water for cement hydration, making the cement slurry hydration more thorough, reducing the self-shrinkage, and the defoaming agent in the concrete can destroy the surface tension of the concrete and prevent bubbles from being generated in the concrete; the surfactant in the defoaming agent can form a lubricating film in the concrete, allowing the concrete particles to slide against each other, thereby improving the compactness of the concrete.
[0098] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A high performance low shrinkage concrete with lightweight aggregate, characterized in that: The concrete is mixed with the following raw materials in percentage by weight: Cement 19%-21%, fly ash 4%-6%, silica fume 12%-15%, water 5%-8%, crushed stone 28%-32%, expanded clay 5%-10%, river sand 15%-20%, 900 grade shale expanded clay 5%-10%, water reducer 5%, and defoaming agent 0.01%.
2. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The cement is 42.5 ordinary Portland cement.
3. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The fly ash is primary fly ash.
4. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The specific surface area of the silica fume is ≥19000m2 / kg, wherein the SiO2 content is ≥90%.
5. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The crushed stone is basalt crushed stone with a particle size of 5-10 mm and a continuous gradation.
6. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The ceramsite is fly ash ceramsite with a bulk density of 1600kg / m3 to 1800kg / m 3 It is composed of 5-12mm size, with a cylinder pressure strength of 13.1MPA, 1h water absorption rate of 4.8%, softening coefficient of 0.9, and the sum of breakage rate and wear rate of 3.1%.
7. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The river sand is medium sand with a fineness modulus of 2.3-2.
6.
8. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The shale ceramic sand is grade 900, with a bulk density of 900kg / m3 to 1400kg / m 3 It is composed of large, medium and small sizes of 0.5-0.35mm, 0.35-0.25mm, and 0.160-0.25, and the weight ratio of large, medium and small sizes of shale ceramic sand is 60-65:20-25:10-20. The cylinder pressure strength is greater than 5MPA, and the chemical composition is mainly silicon dioxide, aluminum oxide, iron oxide, and calcium oxide.
9. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer.
10. The high performance low shrinkage concrete with lightweight aggregate according to claim 1, characterized in that: The main component of the defoamer is modified organic silicon.
11. The method for preparing high-performance low-shrinkage concrete with lightweight aggregate according to any one of claims 1 to 10, characterized in that: The steps include: S1, pre-wetting the ceramsite to obtain pre-wet ceramsite; S2, stirring water and the admixture to obtain a first mixture; S3, adding the cement, primary fly ash, silica fume and fine aggregate into a forced mixer and dry mixing for 1-2 minutes to uniformly mix the cementitious material and the fine aggregate to obtain a second mixture; S4, uniformly mix the first mixture and the second mixture, add coarse aggregate into the mixing equipment and stir for 1-2 minutes, so that the coarse aggregate can be well wrapped by the mortar, and the concrete can be formed; S5, forming the concrete in a mold and performing moisture-keeping curing.
Citation Information
Patent Citations
Lightweight high-strength concrete as well as preparation method and application thereof
CN112266210A
Lightweight high-strength concrete for civil engineering
CN112341121A
Lightweight high-strength concrete and preparation method thereof
CN112521095A
Self-compacting coral lightweight concrete and preparation method thereof
CN112592125A
High-crack-resistance light-weight high-strength self-compacting concrete and preparation method thereof
CN112960952A