A micro-foamed biodegradable film and preparation method thereof

By adding surface modifiers and foaming agents to traditional biodegradable plastics, foam composite materials are formed, which solves the problem of poor compatibility between inorganic fillers and base materials and improves the mechanical properties and degradability of micro-foamed biodegradable films. , achieving an environmentally friendly and economical solution.

CN116285239BActive Publication Date: 2024-10-29DAWN ZHOUSHI (QINGDAO) MULTI LAYER PACKAGING MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310029246.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-10-29
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The inorganic fillers in traditional biodegradable plastics have poor compatibility with the base material, resulting in uneven dispersion and insufficient mechanical properties, making it difficult to completely degrade in the environment.

Method used

Using PBAT as the main raw material, combined with surface modifiers, foaming agents and foaming assistants, foaming composite materials are formed through high-temperature mixing to enhance the compatibility of inorganic fillers and PBAT, and through silane coupling agents and boric acid-containing compounds Improve dispersion and mechanical properties.

Benefits of technology

The tensile strength and melt processability of the micro-foamed biodegradable film are improved, the cost is reduced, and complete biodegradability and environmental protection are achieved. It is suitable for applications such as shopping bags and garbage bags.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004046381940000061
    Figure BDA0004046381940000061
  • Figure BDA0004046381940000071
    Figure BDA0004046381940000071
  • Figure BDA0004046381940000091
    Figure BDA0004046381940000091
Patent Text Reader

Abstract

The present application relates to the field of polymer materials, and specifically discloses a micro-foamed biodegradable film and a preparation method thereof. The micro-foamed biodegradable film includes the following raw materials in parts by weight: 51-79.7 parts of PBAT, 20-45 parts of foamed composite materials, 0.1-2 parts of melt enhancers, 0.1-1 parts of anti-aging agents, and 0.1-1 parts of dispersants; the foamed composite material is mixed with 92-99.2 parts by weight of inorganic fillers, 0.2-2 parts by weight of surface modifiers, 0.5-5 parts by weight of foaming agents, and 0.1-1 parts by weight of foaming aids and heated to 85-110°C. The micro-foamed biodegradable film of the present application has the advantages of being completely biodegradable, good compatibility of inorganic fillers with matrix resins, low cost, high mechanical strength, and strong barrier properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and more specifically, to a micro-foamed biodegradable film and a preparation method thereof. Background Art

[0002] Traditional foam plastics include polyethylene, polypropylene, polyvinyl chloride, polystyrene, etc. Although they are excellent in light weight, heat insulation, sound insulation, cushioning, etc., they are not degradable plastics. After use, they are almost indecomposable in the natural environment. After incineration, they produce a large amount of toxic and harmful gases, which seriously pollute the natural environment. The large-scale use of these foam materials and their non-degradability have brought great pressure to the environment. Therefore, the preparation of biodegradable foam materials has become an urgent problem to be solved by the whole society.

[0003] Polylactic acid (PLA), polybutylene succinate (PBS), poly (butylene terephthalate-co-butylene adipate) ester (PBAT), polyhydroxyalkanoate (PHA) etc. can be fully biodegraded, discarded in nature after use, and can be fully degraded into water and carbon dioxide under the action of microorganisms. Therefore, it can be widely used in the field of plastic films to reduce the pollution to the environment caused by the use of traditional films. However, the above biodegradable materials are priced higher, and the prepared films are less competitive in price compared with traditional ones. Inorganic fillers are abundant in nature and low in price. Adding them to the above-mentioned biodegradable plastics can not only improve the performance of the material, but also greatly reduce the cost of the material, and promote its promotion and use.

[0004] With respect to the above-mentioned related technologies, the inventors found that if inorganic fillers are directly added to biodegradable plastics, the inorganic fillers and the base material are mixed more in a simple physical blending manner, lacking reactive blending between the components, resulting in poor compatibility between the organic components and the inorganic fillers, making it difficult for the inorganic fillers to be evenly dispersed in the matrix, and the inorganic fillers are easy to agglomerate and have poor dispersion, which ultimately leads to problems such as insufficient mechanical properties of the film. Summary of the invention

[0005] In order to improve the compatibility of inorganic fillers with degradable substrates, increase the dispersibility of inorganic fillers in degradable substrates, and enhance the mechanical properties of micro-foamed films, the present application provides a micro-foamed biodegradable film and a preparation method thereof.

[0006] In a first aspect, the present application provides a micro-foamed biodegradable film, which adopts the following technical solution:

[0007] A micro-foamed biodegradable film comprises the following raw materials in parts by weight: 51-79.7 parts of PBAT, 20-45 parts of foamed composite material, 0.1-2 parts of melt enhancer, 0.1-1 parts of anti-aging agent, and 0.1-1 parts of dispersant;

[0008] The preparation method of the foamed composite material is as follows: 92-99.2 parts of inorganic filler, 0.2-2 parts of surface modifier, 0.5-5 parts of foaming agent and 0.1-1 parts of foaming aid are mixed and stirred, and the mixture is heated to 85-110° C. to obtain the foamed composite material.

[0009] By adopting the above technical scheme, PBAT is used as the main raw material, which is completely biodegradable and also has high flexibility, excellent impact strength and melt processability. The melt enhancer is used to increase the melt strength, so that the bubbles can be wrapped without melt fracture, bubble combination and collapse when preparing the micro-foamed biodegradable film. The inorganic filler is treated with a surface modifier to enhance the compatibility between the inorganic filler and PBAT. Moreover, when the inorganic filler and the surface modifier are mixed, a foaming agent and a foaming aid are also added. When the surface modifier modifies the surface of the inorganic filler, it can also modify the foaming agent and the foaming aid, enhance the dispersion uniformity of the foaming aid and the foaming agent and PBAT, make the pores in the biodegradable film uniform, and thus improve the mechanical properties such as tensile strength.

[0010] Optionally, the surface modifier is a silane coupling agent or a boric acid-containing organic compound.

[0011] By adopting the above technical scheme, the silane coupling agent can produce a chemical effect on the surface of the inorganic filler during surface treatment. Through two types of groups, one end is combined with the surface of the inorganic filler and the other end reacts with the PBAT resin through chemical reactions or physical and chemical reactions, thereby making the inorganic filler and PBAT better compatible; the boric acid-containing organic compound uses the boron atom as the central atom, which can improve the compatibility between the inorganic filler and PBAT, thereby improving the mechanical strength of the micro-foamed biodegradable film.

[0012] Optionally, the silane coupling agent is selected from at least one of an aminosilane coupling agent, a carboxyl silane coupling agent and an epoxy silane coupling agent;

[0013] The boric acid-containing compound is selected from at least one of phenylboric acid, 1,4-phenylenediboric acid, 4-vinylphenylboric acid and tetraphenylboric acid.

[0014] By adopting the above technical scheme, aminosilane coupling agent, epoxysilane coupling agent, phenylboric acid, etc. are used as surface modifiers to effectively improve the dispersibility between inorganic fillers and PBAT, reduce the agglomeration of inorganic fillers, and improve the tensile strength and other mechanical properties of the micro-foamed biodegradable film.

[0015] Optionally, the anti-aging agent includes a light stabilizer and a UV absorber in a mass ratio of 1:1-3;

[0016] The light stabilizer is at least one of hexamethylphosphoric triamide, 2,4,6-tris(2'-hydroxy-4'-n-butoxyphenyl)-1,3,5-triazine, and tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite;

[0017] The ultraviolet absorber is at least one of 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole.

[0018] By adopting the above technical scheme, the light stabilizer and the ultraviolet absorber can enhance the light aging resistance and heat aging resistance of the micro-foamed biodegradable film.

[0019] Optionally, the melt enhancer is selected from one of polycarbodiimide, polyisocyanate and 1,4-butanediol diacrylate.

[0020] By adopting the above technical solution, polycarbodiimide and the like are used as melt enhancers to increase melt strength, prevent bubble collapse and merging during foaming, and thus affect the uniformity of the pores of the micro-foamed biodegradable film.

[0021] Optionally, the inorganic filler is at least one of calcium carbonate, wollastonite, kaolin and talc.

[0022] Optionally, the foaming agent is at least one of ammonium carbonate, sodium bicarbonate, benzenesulfonyl hydrazide and urea;

[0023] The foaming aid is at least one of zinc oxide, lauric acid, barium sulfate and potassium aluminum sulfate.

[0024] Optionally, the micro-foamed biodegradable film also includes 15-25 parts by weight of a barrier modifier, and the barrier modifier includes the following components in parts by weight: 5-10 parts of PPC, 1-3 parts of okra straw fiber, 1-3 parts of eggshell membrane, 0.8-1.5 parts of corn oil, 3-5 parts of polyvinyl alcohol, 0.4-0.8 parts of nano α-Fe2O3, and 0.04-0.08 parts of emulsifier.

[0025] By adopting the above technical solution, when the micro-foam biodegradable film is used for food packaging, there are problems such as weak barrier properties and poor sealing properties. Therefore, a barrier modifier is used to improve the barrier ability of the micro-foam biodegradable film to water vapor and oxygen, thereby extending the shelf life of food.

[0026] Okra straw is widely available, has abundant reserves, and is low in cost. It is also hard in texture and difficult to return to the fields. Incineration will cause environmental pollution and waste of resources. Therefore, using okra straw to extract okra straw fiber can save resources and reduce environmental pollution. Okra straw fiber has good mechanical properties, but it is hygroscopic. The main components of corn oil are palmitic acid, oleic acid, and linoleic acid, which are characterized by good water resistance. Therefore, it can improve the water resistance of okra straw fiber and reduce its hygroscopicity. Eggshell membrane is a natural biomass resource and a sustainable renewable biomaterial. It is insoluble in water and has good stability. It is composed of highly cross-linked protein fibers and presents a three-dimensional layered porous network structure. It can extend the permeation path of water vapor and oxygen and increase the barrier property. PPC is a fat polymerized by carbon dioxide and propylene oxide under the action of a catalyst. The polycarbonate of the family has a tightly arranged molecular chain and has the characteristics of good gas barrier property, biodegradability and good flexibility. Moreover, when okra straw fiber and PPC are mixed with a foaming agent, okra straw fiber and PPC can also produce foaming behavior. Nano-α-Fe2O3 can play the role of a nucleating agent, which increases the number of foaming holes of okra straw fiber and PPC, reduces the pore size, and improves the foaming ratio. Moreover, nano-α-Fe2O3 has photocatalytic properties and has a good antibacterial effect on pathogens, which can improve the antibacterial effect of micro-foaming biodegradable film. In addition, nano-α-Fe2O3 can effectively improve the utilization rate of light, and the products of the redox reaction are carbon dioxide and water, which are harmless to the environment. Moreover, nano-α-Fe2O3 can also form chemical bonds with the hydroxyl groups on polyvinyl alcohol, and improve the barrier property of the degradable film by affecting the hydroxyl function on the surface of polyvinyl alcohol.

[0027] Optionally, the preparation method of the barrier modifier is as follows:

[0028] Dissolve polyvinyl alcohol to prepare polyvinyl alcohol aqueous solution, disperse nano-α-Fe2O3 in anhydrous ethanol, and perform ultrasonic treatment for 15-20 minutes to prepare nano-dispersion liquid;

[0029] Mix corn oil and emulsifier, raise the temperature to 40-45° C., stir evenly, add the polyvinyl alcohol aqueous solution and the nano-dispersion liquid, stir at 30-40° C. for 50-60 minutes, and prepare a mixed emulsion;

[0030] The mixed emulsion is mixed evenly with eggshell membrane and okra straw fiber, dried at 60-65° C. for 1.5-2 hours, mixed with PPC, extruded, and granulated.

[0031] By adopting the above technical scheme, the eggshell membrane is insoluble in water, has good stability, is mainly composed of protein fibers, has a strippable double-layer structure, many protein amino acid residues are exposed on the fiber surface, so the functional groups are rich, and the fibers are interpenetrated into a network pore structure, which provides a large area for the loading of nano-α-Fe2O3, and the nano-α-Fe2O3 has a high specific surface area, there are more atoms on the surface, and there are no adjacent atoms around these atoms, resulting in many empty bonds, most bond states lose pairing, and the number of active centers increases, so that the nano-α-Fe2O3 has a high adsorption capacity and can be highly adsorbed on the surface of the eggshell membrane. The adhesion of polyvinyl alcohol can further enhance the loading fastness of nano-α-Fe2O3 and eggshell membrane, and nano-α-Fe2O3 can improve the antibacterial property of the eggshell membrane, and nano-α-Fe2O3 can bind to the hydroxyl groups on the surface of polyvinyl alcohol. The nano-α-Fe2O3 is loaded on the okra straw fiber. When the okra straw fiber and PPC are foamed after being blended with PBAT, they can act as a nucleating agent on the okra straw fiber, which increases the number of okra straw fiber pores and reduces the pore size. The okra straw fiber and nano-α-Fe2O3 form a fiber mesh skeleton structure. Nano-α-Fe2O3 is uniformly adsorbed on the fiber mesh skeleton structure, making the pore surface smoother. Nano-α-Fe2O3 forms hydrogen bonds with the hydroxyl groups on the polyvinyl alcohol attached to the surface of the okra straw, which can further improve the barrier properties of the okra straw fiber. In addition, corn oil and polyvinyl alcohol with a reduced number of hydroxyl groups are hydrophobic, which can improve the compatibility of eggshell membrane and okra straw fiber with PPC, reduce the water absorption rate of eggshell membrane and okra straw fiber, and improve the barrier properties.

[0032] In a second aspect, the present application provides a method for preparing a micro-foamed biodegradable film, using the following technical solution: A method for preparing a micro-foamed biodegradable film, comprising the following steps:

[0033] The PBAT, foamed composite material, melt enhancer, anti-aging agent and dispersant are uniformly mixed to obtain a raw material mixture; the raw material mixture is melted, extruded and granulated to obtain blown film resin particles;

[0034] The blown film resin particles are subjected to film blowing to form a micro-foamed biodegradable film.

[0035] By adopting the above technical scheme, after the raw materials are mixed, they are made into a degradable film through melting, extrusion, granulation and blow molding. The preparation method is simple and easy, the equipment requirements are simple, and it is conducive to large-scale production and application in the market.

[0036] In summary, this application has the following beneficial effects:

[0037] 1. Since the present application mixes the inorganic filler with the surface modifier, the foaming agent and the foaming aid at high temperature to obtain the foamed composite material, the technical problem of poor compatibility between the inorganic filler and the resin is solved, the cost is low, the aging resistance is excellent, and the product can be completely degraded after use without causing any pollution to the environment. It meets the requirements of green environmental protection and can be used for shopping bags, garbage bags, ziplock bags, etc.

[0038] 2. In the present application, it is preferred to add a barrier modifier to the micro-foamed biodegradable film, and the barrier modifier is made of components such as nano α-Fe2O3, okra straw fiber, eggshell membrane, corn oil, polyvinyl alcohol and PPC. Corn oil can reduce the hygroscopicity of okra straw fiber, polyvinyl alcohol can increase the load fastness of nano α-Fe2O3, eggshell membrane and okra straw fiber, and nano α-Fe2O3 can form hydrogen bonds with the hydroxyl groups on polyvinyl alcohol to reduce the hydrophilicity of polyvinyl alcohol and improve the waterproof barrier properties. It also acts as a nucleating agent when the okra straw fiber and PPC are foamed to increase the number of bubbles and increase the buffering capacity. DETAILED DESCRIPTION

[0039] Preparation Examples 1-7 of Barrier Modifiers

[0040] Preparation Example 1: 5 kg of polyvinyl alcohol was dissolved to prepare a polyvinyl alcohol aqueous solution with a concentration of 5 wt %, 0.4 kg of nano-α-Fe2O3 was dispersed in 50 ml of anhydrous ethanol, and the mixture was ultrasonicated for 15 min at a power density of 65 W / L to prepare a nano-dispersion liquid; 1.5 kg of corn oil and 0.08 kg of an emulsifier were mixed, the mixture was heated to 45° C., stirred evenly, the polyvinyl alcohol aqueous solution and the nano-dispersion liquid were added, and the mixture was stirred at 40° C. for 50 min to prepare a mixed emulsion, wherein the emulsifier was monoglyceride;

[0041] The mixed emulsion was mixed evenly with 3 kg of eggshell membrane and 3 kg of okra straw fiber, dried at 60 ° C for 2 h, and mixed with 10 kg of PPC mixing, extrusion and granulation at 165°C. The eggshell membrane is prepared by breaking fresh eggs, tearing off the eggshell membrane attached to the eggshell, thoroughly washing the obtained eggshell membrane in double distilled water to remove the adhered egg white, vacuum drying at room temperature, and then cutting the membrane into 5mm×8mm rectangular blocks. Okra straw fiber is prepared by the following method: peeling okra straw to obtain straw skin, heating the straw skin in 2.5g / L hydrochloric acid at 60°C in a water bath for 2h, washing with water, and scouring with 15wt% sodium hydroxide for 3h, washing with water, and boiling with 1.5g / L hydrogen peroxide and 3g / L alkali solution (composed of caustic soda, soda ash and sodium silicate in a mass ratio of 1:2:1) at 95°C for 30min, and then scouring with 5wt% sodium hydroxide and 2wt% sodium carbonate at 100°C for 2h, washing with water, and drying.

[0042] Preparation Example 2: 3 kg of polyvinyl alcohol was dissolved to prepare a polyvinyl alcohol aqueous solution with a concentration of 3 wt%, 0.8 kg of nano-α-Fe2O3 was dispersed in 50 ml of anhydrous ethanol, and ultrasonicated for 20 min at a power density of 60 W / L to prepare a nano-dispersion liquid;

[0043] 0.8 kg corn oil and 0.04 kg emulsifier were mixed, heated to 40° C., stirred evenly, the polyvinyl alcohol aqueous solution and the nano-dispersion were added, and stirred at 30° C. for 60 min to obtain a mixed emulsion, wherein the emulsifier was sucrose ester;

[0044] The mixed emulsion was mixed evenly with 1 kg of eggshell membrane and 1 kg of okra straw fiber, dried at 65°C for 1.5 h, and then mixed with 5 kg of PPC mixing, extrusion and granulation at 165°C. The eggshell membrane is prepared by breaking fresh eggs, tearing off the eggshell membrane attached to the eggshell, thoroughly washing the obtained eggshell membrane in double distilled water to remove the adhered egg white, vacuum drying at room temperature, and then cutting the membrane into 5mm×8mm rectangular blocks. Okra straw fiber is prepared by the following method: peeling okra straw to obtain straw skin, heating the straw skin in 2.5g / L hydrochloric acid at 60°C in a water bath for 2h, washing with water, and scouring with 15wt% sodium hydroxide for 3h, washing with water, and boiling with 1.5g / L hydrogen peroxide and 3g / L alkali solution (composed of caustic soda, soda ash and sodium silicate in a mass ratio of 1:2:1) at 95°C for 30min, and then scouring with 5wt% sodium hydroxide and 2wt% sodium carbonate at 100°C for 2h, washing with water, and drying.

[0045] Preparation Example 3: The difference from Preparation Example 1 is that no nano-dispersion liquid containing nano-α-Fe2O3 is added.

[0046] Preparation Example 4: The difference from Preparation Example 1 is that corn oil is not added.

[0047] Preparation Example 5: The difference from Preparation Example 1 is that eggshell membrane is not added.

[0048] Preparation Example 6: The difference from Preparation Example 1 is that no PPC is added.

[0049] Preparation Example 7: The difference from Preparation Example 1 is that okra straw fiber is not added.

[0050] Example

[0051] Example 1: A micro-foamed biodegradable film, the amount of raw materials used is shown in Table 1, wherein the melt index of PBAT is 5g / 10min, the melt enhancer is polycarbodiimide, the anti-aging agent includes a light stabilizer and a UV absorber in a mass ratio of 1:3, the light stabilizer is hexamethylphosphoric triamide, the UV absorber is 2-(2'-hydroxy-3', 5'-di-tert-phenyl)-5-chlorobenzotriazole, the dispersant is polyethylene wax, and the composite foaming material includes 99.2kg of inorganic filler, 2kg of surface modifier, 5kg of foaming agent and 1kg of foaming aid, wherein the inorganic filler is calcium carbonate with a particle size of 800 mesh, the surface modifier is Dow Corning 6121 aminosilane coupling agent and KH560 epoxy silane coupling agent in a mass ratio of 1:1, the foaming agent is ammonium carbonate, and the foaming aid is zinc oxide.

[0052] The method for preparing the micro-foamed biodegradable film comprises the following steps:

[0053] S1, mixing an inorganic filler, a surface modifier, a foaming agent and a foaming aid, adding the mixture into a high-speed mixer with a heating device, mixing at a speed of 1200 rpm and heating to 110° C. to obtain a foamed composite material;

[0054] S2, stirring PBAT, foaming composite material, melt enhancer, anti-aging agent and dispersant at a speed of 150 rpm for 2 min, and then stirring at a speed of 1300 rpm for 3 min, mixing well to obtain a raw material mixture;

[0055] S3, melting, extruding and granulating the raw material mixture at 150° C. to obtain blown film resin particles, with a screw speed of 80 rpm;

[0056] S4. Forming a film by blowing the film-blowing resin particles to obtain a micro-foamed biodegradable film with a thickness of 0.08 mm, the film blowing temperature being 180° C. and the screw speed being 30 rpm.

[0057] Table 1 Raw material dosage of micro-foamed biodegradable film in Examples 1-4

[0058]

[0059] Table 2 Amount of raw materials used in the foamed composite materials in Examples 1-4

[0060]

[0061] Example 2-4: A micro-foamed biodegradable film, which is different from Example 1 in that the amounts of raw materials used are as shown in Table 1, wherein the amounts of raw materials used for the foamed composite material are as shown in Table 2.

[0062] Example 5: A micro-foamed biodegradable membrane, which is different from Example 1 in that the surface modifier is Dow Corning 6121 aminosilane coupling agent.

[0063] Example 6: A micro-foamed biodegradable film, which is different from Example 1 in that the surface modifier is an organic compound containing boric acid, and the organic compound containing boric acid is 1,4-phenylboric acid.

[0064] Example 7: A micro-foamed biodegradable film, which is different from Example 1 in that the surface modifier is a boric acid-containing organic compound, and the boric acid-containing organic compound includes phenylboric acid, 4-vinylphenylboric acid and tetraphenylboric acid in a mass ratio of 1:0.3:0.7.

[0065] Example 8: A micro-foamed biodegradable film, which differs from Example 1 in that, in step S1, 25 kg of the barrier modifier prepared in Preparation Example 1 is mixed with PBAT, a foamed composite material, a melt enhancer, an anti-aging agent and a dispersant to obtain a raw material mixture.

[0066] Example 9: A micro-foamed biodegradable film, which differs from Example 1 in that, in step S1, 15 kg of the barrier modifier prepared in Preparation Example 2 is mixed with PBAT, a foamed composite material, a melt enhancer, an anti-aging agent and a dispersant to obtain a raw material mixture.

[0067] Example 10: A micro-foamed biodegradable film, which is different from Example 8 in that the barrier modifier is made from Preparation Example 3.

[0068] Example 11: A micro-foamed biodegradable film, which is different from Example 8 in that the barrier modifier is made from Preparation Example 4.

[0069] Example 12: A micro-foamed biodegradable film, which is different from Example 8 in that the barrier modifier is made from Preparation Example 5.

[0070] Example 13: A micro-foamed biodegradable film, which is different from Example 8 in that the barrier modifier is made from Preparation Example 6.

[0071] Example 14: A micro-foamed biodegradable film, which is different from Example 8 in that the barrier modifier is made from Preparation Example 7.

[0072] Comparative Example

[0073] Comparative Example 1: A micro-foamed biodegradable film, which is different from Example 1 in that the foamed composite material is prepared by mixing 99.2 kg of inorganic filler, 2 kg of surface modifier, 5 kg of foaming agent and 1 kg of foaming aid at room temperature.

[0074] Comparative Example 2: A micro-foamed biodegradable film, which is different from Example 1 in that no surface modifier is added to the foamed composite material.

[0075] Comparative Example 3: A micro-foamed biodegradable film, which differs from Example 1 in that no melt enhancer is added.

[0076] Comparative Example 4: A method for preparing a micro-foamed degradable mulch film, comprising the following steps:

[0077] The first step: 100 parts of degradable polymer PBAT, 2.5 parts of microbubble forming agent (the mass ratio of azodicarbonamide to zinc sulfate heptahydrate is 5:1), 2 parts of tear resistant agent (prepare tear resistant agent according to the mass proportion of 10 parts of dicumyl peroxide, 25 parts of 2-hydroxypropyl-β-cyclodextrin, 8 parts of inositol hexaphosphate, 9 parts of disulfide carbamate, 10 parts of sodium alginate and 20 parts of cellulose acetate butyrate. Specifically, dicumyl peroxide is dissolved in an organic solvent to obtain a dicumyl peroxide solution. The amount of organic solvent used is Completely dissolve dicumyl peroxide without precipitation; mix the obtained dicumyl peroxide solution with 2-hydroxypropyl-β-cyclodextrin evenly without lumps; add the remaining materials to the mixture, mix evenly without lumps), add 3 parts of microbubble homogenizer (1 part of ethylene bisstearamide and 2 parts of oxidized polyethylene wax) to a high-speed mixer, first mix at 60 rpm for 15 minutes, then heat to 60°C and mix at 1000 rpm for 20 minutes to obtain a PBAT premix.

[0078] Step 2: Add the PBAT premix prepared in the first step into a twin-screw extruder for melt extrusion reaction at an extrusion temperature of 135°C and a screw speed of 80 rpm to prepare a PBAT micro-foamed mulch film special material.

[0079] Step 3: Use a film blowing machine to foam and blow the PBAT micro-foamed ground film material prepared in the second step. The film blowing temperature is set to 155°C and the screw speed is 25rpm.

[0080] Performance testing

[0081] The micro-foam film was prepared according to the methods in the examples and comparative examples, and the properties of the micro-foam film were tested according to the following methods. The test results are recorded in Table 3.

[0082] 1. Tensile strength and elongation at break: GB / T1040.3-2006 "Determination of tensile properties of plastics Part 3: Films and sheets" for testing;

[0083] 2. Degradation rate: 1. Degradation rate: Take the same mass of the micro-foam films prepared in each embodiment and comparative example, bury them 10 cm below the surface of the compost soil, the compost soil is the soil for cultivating flowers in the natural environment, and then add water quantitatively every 3 days to ensure that the degradation environment is humid. On the 120th day, take out the micro-foam film, rinse it, dry it in a 50°C oven and weigh it, and calculate the weight loss rate, which is degradation rate (%) = (mass before degradation - mass after degradation) / mass before degradation × 100%;

[0084] 3. Water vapor transmission rate: According to GB / T26253-2010 "Determination of water vapor transmission rate of plastic film and sheeting - Infrared detector method", the test was carried out using a BASIC301 water vapor transmission rate tester at a temperature of 23°C and a relative humidity of 85%;

[0085] 4. Oxygen permeability: The test was conducted using a VACV1 oxygen permeability tester at a temperature of 23°C and a relative humidity of 0%.

[0086] Table 3 Performance test results of micro-foamed biodegradable membrane

[0087]

[0088] The amounts of the foamed composite materials used in Examples 1-4 are different, and the amounts of the raw materials used in the micro-foamed biodegradable films are different. The inorganic fillers of the biodegradable films prepared thereby have good compatibility with PBAT, high tensile strength, large elongation at break, and a degradation rate of more than 80% within 120 days, with a fast degradation rate.

[0089] Compared with Example 1, the tensile strength, elongation at break and other properties of the micro-foamed biodegradable film prepared by using aminosilane coupling agent alone as the surface modifier are similar to those of Example 1.

[0090] In Example 6, 1,4-phenylboric acid was used as a surface modifier, and in Example 7, phenylboric acid, 4-vinylphenylboric acid and tetraphenylboric acid were used as surface modifiers. The performance of the micro-foamed biodegradable films prepared in Examples 6 and 7 was not much different from that in Example 1.

[0091] Compared with Example 1, Example 8 and Example 9 further added a barrier modifier. The data in Table 3 showed that the tensile strength and elongation at break of the micro-foamed biodegradable films prepared in Example 8 and Example 9 were increased, and the barrier properties to water vapor and oxygen were enhanced, and the degradation rate did not change much, indicating that the addition of the barrier modifier can improve the mechanical strength of the film while increasing the barrier properties of the micro-foamed biodegradable film.

[0092] In Example 10, the barrier modifier prepared in Preparation Example 3 was used. In Preparation Example 3, no nano-dispersion containing nano-α-Fe2O3 was added. Compared with Example 8, Table 3 shows that the oxygen permeability and water vapor permeability of the micro-foamed biodegradable film prepared in Example 10 increased, and the barrier property decreased.

[0093] Compared with Example 8, Example 11 uses the barrier modifier prepared in Preparation Example 4 without adding corn oil. The barrier property of the micro-foamed biodegradable film prepared in Example 11 to water vapor and oxygen is weakened, and the mechanical strength is slightly reduced.

[0094] In Example 12, a barrier modifier made without adding eggshell membrane was used. As shown in Table 3, the barrier ability of the micro-foamed biodegradable film to water vapor and oxygen was weakened, and the tensile strength and elongation at break decreased.

[0095] Compared with Example 8, Example 13 uses the barrier modifier prepared in Preparation Example 6, in which no PPC is added. The mechanical strength and barrier properties of the micro-foamed biodegradable film prepared in Example 13 are reduced.

[0096] In Example 14, no okra straw fiber was added to the barrier modifier. Compared with Example 8, the tensile strength of the micro-foamed biodegradable film prepared in Example 14 was weakened, the mechanical properties deteriorated, and the barrier properties improved, indicating that okra straw has moisture absorption and moisture permeability and needs to be used in combination with corn oil and nano α-Fe2O3.

[0097] Compared with Example 1, the foamed composite material in Comparative Example 1 was not treated at high temperature, and no surface modifier was added to the foamed composite material in Comparative Example 2. The tensile strength and elongation at break of the micro-foamed biodegradable films prepared in Comparative Example 1 and Comparative Example 2 were significantly reduced, and the other properties were not much different from those in Example 1.

[0098] In Comparative Example 3, no melt enhancer was added. Compared with Example 1, the tensile strength and elongation at break of the micro-cellular biodegradable film prepared in Comparative Example 3 decreased, and the mechanical properties weakened.

[0099] Comparative Example 4 is a degradable mulch film prepared using raw materials such as PBAT, tear resistant agent, and microbubble forming agent. Its mechanical strength, biodegradation rate, and barrier properties are all inferior to those of Example 1.

[0100] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A micro-foamed biodegradable film, characterized in that: The invention comprises the following raw materials in parts by weight: 51-79.7 parts of PBAT, 20-45 parts of foaming composite material, 0.1-2 parts of melt enhancer, 0.1-1 parts of anti-aging agent, 0.1-1 parts of dispersant, and 15-25 parts of barrier modifier; The foamed composite material is prepared by mixing 92-99.2 parts by weight of an inorganic filler, 0.2-2 parts by weight of a surface modifier, 0.5-5 parts by weight of a foaming agent, and 0.1-1 parts by weight of a foaming aid and heating the mixture to 85-110° C.; The barrier modifier comprises the following components in parts by weight: 5-10 parts of PPC, 1-3 parts of okra straw fiber, 1-3 parts of eggshell membrane, 0.8-1.5 parts of corn oil, 3-5 parts of polyvinyl alcohol, 0.4-0.8 parts of nano α-Fe2O3, and 0.04-0.08 parts of emulsifier; The preparation method of the barrier modifier is as follows: Dissolve polyvinyl alcohol to prepare polyvinyl alcohol aqueous solution, disperse nano-α-Fe2O3 in anhydrous ethanol, and perform ultrasonic treatment for 15-20 minutes to prepare nano-dispersion liquid; Mix corn oil and emulsifier, raise the temperature to 40-45° C., stir evenly, add the polyvinyl alcohol aqueous solution and the nano-dispersion liquid, stir at 30-40° C. for 50-60 minutes, and prepare a mixed emulsion; The mixed emulsion is mixed evenly with eggshell membrane and okra straw fiber, dried at 60-65° C. for 1.5-2 hours, mixed with PPC, extruded, and granulated.

2. The micro-foamed biodegradable film according to claim 1, characterized in that: The surface modifier is a silane coupling agent or a boric acid-containing organic compound.

3. The micro-foamed biodegradable film according to claim 2, characterized in that: The silane coupling agent is selected from at least one of an aminosilane coupling agent, a carboxyl silane coupling agent and an epoxy silane coupling agent; The boric acid-containing compound is selected from at least one of phenylboric acid, 1,4-phenylenediboric acid, 4-vinylphenylboric acid and tetraphenylboric acid.

4. The micro-foamed biodegradable film according to claim 1, characterized in that: The anti-aging agent includes a light stabilizer and a UV absorber in a mass ratio of 1:1-3; The light stabilizer is at least one of hexamethylphosphoric triamide, 2,4,6-tris(2'-hydroxy-4'-n-butoxyphenyl)-1,3,5-triazine, and tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite; The ultraviolet absorber is at least one of 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, 2-hydroxy-4-n-octyloxybenzophenone, and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole.

5. The micro-foamed biodegradable film according to claim 1, characterized in that: The melt enhancer is selected from one of polycarbodiimide, polyisocyanate and 1,4-butanediol diacrylate.

6. The micro-foamed biodegradable film according to claim 1, characterized in that: The inorganic filler is at least one of calcium carbonate, wollastonite, kaolin and talc.

7. The micro-foamed biodegradable film according to claim 1, characterized in that: The foaming agent is at least one of ammonium carbonate, sodium bicarbonate, benzenesulfonyl hydrazide and urea; The foaming aid is at least one of zinc oxide, lauric acid, barium sulfate and potassium aluminum sulfate.

8. The method for preparing the micro-foamed biodegradable film according to any one of claims 1 to 7, characterized in that: The following steps are involved: Evenly mixing PBAT, a foaming composite material, a melt enhancer, an anti-aging agent and a dispersant to obtain a raw material mixture; Melting, extruding and granulating the raw material mixture to obtain blown film resin particles; The blown film resin particles are subjected to film blowing to form a micro-foamed biodegradable film.

Citation Information

Patent Citations

  • Gas-generating agent

    CN102803424A

  • Micro-foaming degradable mulching film and preparation method thereof

    CN109666271A

  • Degradable chemical foaming masterbatch and preparation method thereof

    CN109762309A

  • Foaming master batch and preparation method thereof

    CN113201210A

  • Foaming assistant material and foam-molding method

    US20170342231A1