A concrete protective material and a preparation method thereof
By modifying epoxy resin with cubic cage silsesquioxane and nitrile rubber, combined with the use of titanium powder, the problem of insufficient tensile strength and bonding strength of epoxy resin in concrete surface protection is solved, and the material's durability is improved. Toughness and durability reduce the linear expansion coefficient, avoid cracking and bulging, and improve the overall performance of concrete protective materials.
Patent Information
- Application Number
- CN202310304117.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-27
AI Technical Summary
In concrete surface protection applications, epoxy resin has low tensile strength, high linear expansion coefficient, low bonding strength, and is prone to cracking, peeling, peeling and other problems, which limits its durability and protective performance.
Cubic cage silsesquioxane and nitrile rubber are used to collaboratively modify epoxy resin to reduce the linear expansion coefficient by increasing the thermal decomposition temperature, enhancing toughness and bonding properties, and adding titanium powder during the preparation process to reduce production costs. and improved thixotropic performance.
Significantly improves the tensile strength, impact strength and bonding performance of epoxy resin, reduces the linear expansion coefficient, extends the service life of the material, avoids cracking and bulging, and improves the durability and construction convenience of concrete protective materials sex.
Smart Images

Figure BDA0004146110880000071 
Figure BDA0004146110880000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a concrete protective material and a preparation method thereof. Background Art
[0002] Epoxy resin putty is widely used in repairing defects in concrete buildings due to its advantages of high hardness and good adhesion. However, it also has the disadvantages of poor toughness, high water absorption, poor corrosion resistance, poor deformation ability, and is prone to many problems such as cracking, peeling, and flaking, which lead to reduced protective durability. These defects limit its further application in concrete defect repair and protection with higher durability requirements such as anti-corrosion and stain resistance.
[0003] However, the current problems with epoxy resins are: the bonding strength with concrete is not high enough, and the tensile strength is low. It has poor toughness, high water absorption, poor corrosion resistance, poor deformation ability, and is prone to cracking, peeling, flaking and many other problems. These defects greatly limit the service life of epoxy resins in concrete surface protection applications. When the ambient temperature changes greatly during service, the large difference in linear expansion coefficients can easily lead to a large difference in deformation between the epoxy putty protective layer and the concrete, thereby causing increased stress in the protective layer. When the tensile, compressive and bonding strengths of the coating itself are exceeded, the coating is prone to cracking or bulging. Summary of the invention
[0004] In order to solve the technical problem that epoxy resin has low tensile strength, high linear expansion coefficient and low bonding strength with concrete, the present invention provides a concrete protective material with high tensile strength, low linear expansion coefficient and high bonding strength with concrete.
[0005] The second object of the present invention is to provide a method for preparing a concrete protective material.
[0006] To achieve the above first purpose, the technical solution adopted by the present invention is:
[0007] A concrete protective material, composed of two components A and B mixed in a mass ratio of 5:1, wherein the component A, by weight, consists of the following components: 100 parts of modified epoxy resin, 10-20 parts of diluent, 2-4 parts of thixotropic agent, and 100-150 parts of titanium powder;
[0008] The B component is composed of the following components by weight: 30-35 parts of a curing agent and 3-6 parts of a curing accelerator;
[0009] The modified epoxy resin is a cubic cage silsesquioxane and nitrile rubber synergistically modified epoxy resin. By adopting cubic cage silsesquioxane and nitrile rubber to synergistically modify the epoxy resin, the thermal decomposition temperature of the epoxy resin can be effectively increased. The silsesquioxane isolates the external thermal erosion of the internal matrix of the composite material on the surface of the composite material, and has a toughening and modification effect on the epoxy resin, and its impact strength and tensile strength are improved. At the same time, the synergistic modification of the nitrile rubber can improve the bearing capacity of the resin, improve the bonding performance between the epoxy resin and concrete, and make the resin less likely to crack under the action of mixed shear. The hydroxyl and methoxy groups in the cage structure react with the hydroxyl groups in the epoxy resin. Under the action of the curing agent, cubic cage silsesquioxane and epoxy resin are cross-linked through chemical bonds, which plays a certain role in network dielectricity. The synergistic modification of nitrile rubber can greatly improve the toughness, impact strength and peel strength. When the material is impacted, it can disperse stress and withstand impact to a certain extent, increase the fracture performance of the material, and reduce the linear expansion coefficient. During the service period of concrete surface protection, it is not easy to crack or bulge. By using titanium powder, the linear expansion coefficient can be minimized, and at the same time, the use of thixotropic agents can be reduced, the production cost can be reduced, the thixotropy of the resin can be adjusted, the storage stability of the material can be improved, and the anti-sagging property of the construction can be improved.
[0010] Preferably, the mass ratio of the cubic cage silsesquioxane and the nitrile rubber is 5:7. By using the cubic cage silsesquioxane and the nitrile rubber in a ratio of 5:7 to synergistically modify the epoxy resin, the toughness of the resin can be increased, so that the resin is not prone to cracks under the action of cyclic shear. More preferably, the nitrile rubber with end carboxyl groups and the cubic cage silsesquioxane are synergistically modified with the epoxy resin. When the ratio is 5:7, the interaction and reaction are sufficient, and the rigid-flexible two-phase performance is fully reflected. It has good high temperature resistance, antioxidant performance, chemical stability and lubrication performance. Because the unique terminal carboxyl structure of the nitrile rubber can migrate to the surface and react with the epoxy group, the surface free energy is reduced, thereby improving the corrosion resistance of the polymer, and the three-dimensional cross-linked network structure of the epoxy resin formed can play a good stress dispersion role.
[0011] Preferably, the preparation method of the modified epoxy resin comprises the following steps:
[0012] The cubic cage silsesquioxane and the epoxy resin are mixed and stirred at 80°C and a rate of 800 r / min for 30 minutes, the temperature is raised to 120°C, nitrile rubber and silane coupling agent KH550 are added, and the mixture is stirred at 100°C and a rate of 800 r / min for 40-50 minutes to obtain a modified epoxy resin. The cubic cage silsesquioxane is first blended with the epoxy resin, and finally the carboxyl-terminated nitrile rubber and the silane coupling agent are added. The cage structure is first introduced and then the nitrile rubber and the epoxy resin are blended. The preparation method is simple and convenient to operate. The prepared modified epoxy resin is used for concrete protective materials, which solves the technical problems of low tensile strength of epoxy resin, high linear expansion coefficient and low bonding strength with concrete.
[0013] Preferably, the epoxy resin is any one of bisphenol A epoxy resin or bisphenol F epoxy resin.
[0014] Preferably, the amount of the cubic cage silsesquioxane added is 10-15% of the mass fraction of the epoxy resin.
[0015] Preferably, the thixotropic agent is fumed silica.
[0016] Preferably, the curing agent is methylhexahydrophthalic anhydride, and the curing accelerator is a tertiary amine accelerator.
[0017] Preferably, the particle size of the titanium powder is 800-1000 mesh.
[0018] Preferably, the diluent is any one of phenyl glycidyl ether, propenyl glycidyl ether and butyl glycidyl ether.
[0019] In order to achieve the above second purpose, the technical solution adopted by the present invention is:
[0020] A method for preparing a concrete protective material as described in any one of the above items comprises the following steps:
[0021] S1. Mix the modified epoxy resin, diluent and thixotropic agent in component A in proportion and fully disperse them to obtain a resin prepolymer, add titanium powder to the prepolymer, and perform vacuum degassing to obtain component A;
[0022] S2. Mix the curing agent and curing accelerator of component B in proportion by mechanical stirring for 30-60 minutes, mix them evenly, and perform vacuum degassing to obtain component B;
[0023] S3. Component A obtained in step S1 and component B obtained in step S2 are stored separately at a mass ratio of 5:1.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1. A concrete protective material provided by the present application can effectively increase the thermal decomposition temperature of the epoxy resin by using cubic cage silsesquioxane and nitrile rubber to synergistically modify the epoxy resin. The silsesquioxane isolates the thermal erosion of the external environment on the internal matrix of the composite material on the surface of the composite material, and has a toughening and modification effect on the epoxy resin, and its impact strength and tensile strength are improved. At the same time, the synergistic modification with nitrile rubber can improve the bearing capacity of the resin, improve the bonding performance between the epoxy resin and concrete, and make the resin less likely to crack under the action of mixed shear. The hydroxyl and methoxy groups in the cage structure react with the hydroxyl groups in the epoxy resin. Under the action of the curing agent, the cubic cage silsesquioxane and the epoxy resin are cross-linked through chemical bonds, which plays a certain role in network dielectricity. The synergistic modification with nitrile rubber can greatly improve the toughness, impact strength and peel strength. When the material is impacted, it can play a role in stress dispersion and impact resistance to a certain extent, increase the fracture performance of the material, and reduce the linear expansion coefficient. During the service period of concrete surface protection, it is not easy to crack or bulge.
[0026] 2. The present application provides a method for preparing a concrete protective material. By preparing component A first and then adding titanium powder, the thixotropic properties of the epoxy resin can be improved and the amount of thixotropic agent vapor-phase silica can be reduced. The operation is simple and quick. The prepared components A and B can be mixed and used for concrete protective coating. DETAILED DESCRIPTION
[0027] The specific technical scheme of the present invention is described below in conjunction with specific embodiments 1-3:
[0028] Embodiment 1:
[0029] A method for preparing a concrete protective material comprises the following steps:
[0030] S1. The modified epoxy resin, diluent and thixotropic agent in component A are mixed and fully dispersed according to the proportion in Table 1, and the dispersion speed is controlled at 800 r / min to obtain a resin prepolymer. Titanium powder is added to the prepolymer, and the dispersion speed is controlled at 1200 r / min. The dispersion time is 60 min, and vacuum degassing is performed under a negative pressure of -0.08 MPa to obtain component A;
[0031] S2. Mix the curing agent and curing accelerator of component B by mechanical stirring for 30 min according to the proportion in Table 1, control the dispersion speed at 600 r / min, and perform vacuum degassing under a negative pressure of -0.08 MPa to obtain component B;
[0032] S3. Mix component A obtained in step S1 and component B obtained in step S2 in a mass ratio of 5:1.
[0033] Embodiment 2:
[0034] A method for preparing a concrete protective material comprises the following steps:
[0035] S1. According to the ratio in Table 1, the modified epoxy resin, diluent and thixotropic agent in component A are mixed and fully dispersed, the dispersion speed is controlled at 900 r / min, and a resin prepolymer is obtained. Titanium powder is added to the prepolymer, the dispersion speed is controlled at 1500 r / min, the dispersion time is 60 min, and vacuum degassing is performed under a negative pressure of -0.08 MPa to obtain component A;
[0036] S2. Mix the curing agent and curing accelerator of component B by mechanical stirring for 40 min according to the proportion in Table 1, control the dispersion speed at 700 r / min, and perform vacuum degassing under a negative pressure of -0.08 MPa to obtain component B;
[0037] S3. Mix component A obtained in step S1 and component B obtained in step S2 in a mass ratio of 5:1.
[0038] Embodiment 3:
[0039] A method for preparing a concrete protective material comprises the following steps:
[0040] S1. According to the ratio in Table 1, the modified epoxy resin, diluent and thixotropic agent in component A are mixed and fully dispersed, the dispersion speed is controlled at 1000 r / min, and a resin prepolymer is obtained. Titanium powder is added to the prepolymer, the dispersion speed is controlled at 1600 r / min, the dispersion time is 60 min, and vacuum degassing is performed under a negative pressure of -0.08 MPa to obtain component A;
[0041] S2. Mix the curing agent and curing accelerator of component B by mechanical stirring for 60 min according to the proportion in Table 1, control the dispersion speed at 900 r / min, and perform vacuum degassing under a negative pressure of -0.08 MPa to obtain component B;
[0042] S3. Mix component A obtained in step S1 and component B obtained in step S2 in a mass ratio of 5:1.
[0043] Table 1: Component ratio of concrete protective materials in Examples 1-3
[0044]
[0045] The tensile strength, compressive strength, elongation at break and impact strength of each embodiment and comparative example (commercially available epoxy resin concrete protective material) were tested according to the following standard GB / T2567-2008 "Test method for properties of resin castings", and the bonding properties and thermal expansion coefficient were tested according to DL / T5193-2004 "Technical specification for epoxy resin mortar". The performance test data results are shown in Table 2.
[0046] Table 2: Test results of Examples 1-3 and Comparative Example (commercially available epoxy resin concrete protective material)
[0047]
[0048] It can be seen from the data in Table 2 that the concrete protective material of the present application can significantly improve the tensile strength and elongation at break of epoxy resin used for concrete protective materials. By using cubic cage-type silsesquioxane and nitrile rubber to synergistically modify epoxy resin, the thermal decomposition temperature of epoxy resin can be effectively increased. Silsesquioxane isolates the thermal erosion of the external environment on the internal matrix of the composite material on the surface of the composite material, and has a toughening and modification effect on the epoxy resin, and its impact strength and tensile strength are improved. At the same time, the synergistic modification with nitrile rubber can improve the bearing capacity of the resin, improve the bonding performance between the epoxy resin and concrete, and make the resin less likely to crack under the action of mixed shear. The hydroxyl and methoxy groups in the cage structure react with the hydroxyl groups in the epoxy resin to form a toughening and modification effect. The reaction occurs, and under the action of the curing agent, the cubic cage silsesquioxane and the epoxy resin are cross-linked through chemical bonds, which plays a certain role in network dielectricity, and the synergistic modification of nitrile rubber can greatly improve the toughness, impact strength and peel strength. When the material is impacted, it can disperse the stress and withstand the impact to a certain extent, increase the fracture performance of the material, and reduce the linear expansion coefficient. During the service period of concrete surface protection, it is not easy to crack or bulge. The preparation method thereof, by first preparing component A and finally adding titanium powder, can improve the thixotropic properties of the epoxy resin and reduce the amount of thixotropic agent gas-phase silica. The operation is simple and quick, and the prepared components A and B can be used for concrete protective coating after mixing.
[0049] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A concrete protective material, characterized in that: It is composed of two components A and B mixed in a mass ratio of 5:
1. Component A, by weight, is composed of the following components: 100 parts of modified epoxy resin, 10-20 parts of diluent, 2-4 parts of thixotropic agent, and 100-150 parts of titanium powder; Component B, by weight, consists of the following components: 30-35 parts of curing agent and 3-6 parts of curing accelerator; The modified epoxy resin is a cubic cage silsesquioxane and nitrile rubber synergistically modified epoxy resin; The mass ratio of the cubic cage silsesquioxane to the nitrile rubber is 5:7; The preparation method of the modified epoxy resin comprises the following steps: The cubic cage silsesquioxane and the epoxy resin were mixed and stirred at 80°C and 800 r / min for 30 minutes, the temperature was raised to 120°C, nitrile rubber and silane coupling agent KH550 were added, and the mixture was stirred at 100°C and 800 r / min for 40-50 minutes to obtain a modified epoxy resin; The amount of the cubic cage silsesquioxane added is 10-15% of the mass fraction of the epoxy resin; The cubic cage structure of the cubic cage silsesquioxane contains hydroxyl groups and methoxy groups.
2. The concrete protective material according to claim 1, characterized in that: The epoxy resin is any one of bisphenol A epoxy resin and bisphenol F epoxy resin.
3. The concrete protective material according to claim 1, characterized in that: The thixotropic agent is fumed silica.
4. The concrete protective material according to claim 1, characterized in that: The curing agent is methylhexahydrophthalic anhydride, and the curing accelerator is a tertiary amine accelerator.
5. The concrete protective material according to claim 1, characterized in that: The particle size of the titanium powder is 800-1000 mesh.
6. The concrete protective material according to claim 1, characterized in that: The diluent is any one of phenyl glycidyl ether and butyl glycidyl ether.
7. A method for preparing a concrete protective material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Mix the modified epoxy resin, diluent and thixotropic agent in component A in proportion and fully disperse them to obtain a resin prepolymer, add titanium powder to the prepolymer, and perform vacuum degassing to obtain component A; S2. Mix the curing agent and curing accelerator of component B in proportion by mechanical stirring for 30-60 minutes, mix them evenly, and perform vacuum degassing to obtain component B; S3. Component A obtained in step S1 and component B obtained in step S2 are stored independently at a mass ratio of 5:1.
Citation Information
Patent Citations
Epoxy resin daub for building joint filling and preparation method thereof
CN109517343A
Underwater composite anticorrosive coating and preparation method thereof
CN110172288A
High-strength fatigue-resistant epoxy resin structural adhesive and preparation method thereof
CN110317561A
Microwave curing epoxy resin material for concrete protection and preparation method thereof
CN114921148A
Epoxy resin adhesive for repairing building cracks and preparation method of epoxy resin adhesive
CN115340838A