A production method for high-purity raw material pure iron continuous casting large square billet BGPI99

Through the technological process of ginseng iron + molten iron desulfurization pretreatment + converter smelting + LF furnace refining + RH vacuum treatment + bloom continuous casting, the problem of producing pure iron from high-purity raw materials has been solved, and the production of low-cost, high-purity raw material pure iron has been achieved. Meet the composition requirements of high-end steel materials.

CN116287937BActive Publication Date: 2024-10-18BENGANG STEEL PLATES CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211617805.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-10-18
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively produce high-purity raw material pure iron, resulting in its composition being unable to meet the low requirements for low conventional element and residual element content, and the production process is complex and costly.

Method used

Adopting the technological process of ginseng iron + molten iron desulfurization pretreatment + converter smelting + LF furnace refining + RH vacuum treatment + bloom continuous casting, desulfurization through passivation of magnesium powder and calcium oxide powder, double slag method dephosphorization, manganese removal, and forced desulfurization Carbon and other steps are used to control the composition of molten steel to achieve the production of pure iron as a high-purity raw material.

Benefits of technology

It achieves high-purity and low-cost production of raw material pure iron to meet high-purity requirements. The steel has high purity, low residual element content, and good surface quality of the cast slab, which meets the requirements for the use of high-end steel materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004002028460000051
    Figure BDA0004002028460000051
  • Figure HDA0004002028470000011
    Figure HDA0004002028470000011
Patent Text Reader

Abstract

The present invention provides a method for preparing high-purity raw material pure iron continuous casting large square billet BGPI99, which adopts ginseng iron + molten iron desulfurization pretreatment + converter smelting + LF furnace refining + RH vacuum treatment + large square billet continuous casting. The steel has high purity and low residual element content; the Mn content can be controlled within 0.03% and the P content can be controlled within 0.003%. The surface quality of the casting billet is good, which fully meets the use needs of raw material pure iron customers at home and abroad.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing a metal material, in particular to a method for producing a high-purity raw material pure iron continuous casting large square billet BGPI99. Background Art

[0002] Raw pure iron is an important basic raw material for steel. It is mainly used as a masterbatch for smelting high-end steel materials, and is added with various alloys to produce various heat-resistant alloys, high-temperature alloys, precision alloys, maraging steels and other high-end steel materials for aerospace, military and civilian use. It has developed very rapidly at home and abroad in recent years. The development and production of high-purity raw pure iron can improve the quality grade of raw pure iron, expand the scope of use of raw pure iron, and thus improve the quality of high-end steel materials. However, the preparation process of high-purity raw pure iron in China is not very mature, and the supply of high-purity raw pure iron cannot meet the demand. In terms of composition, the lower the content of industrial pure iron, whether it is conventional elements (C, Si, Mn, P, S) or residual elements (Nb, V, Ti, Ni, Mo, Cu, As, Sn, etc.), the better. Therefore, many companies are pursuing to reduce the content of the above elements to the maximum extent, but it is very difficult to produce high-purity raw pure iron.

[0003] Patent No. CN 108277316 B discloses a method for producing pure iron, which uses a "double desulfurization and double stripping" process to desulfurize molten iron and then uses a converter to smelt it. The composition of the pure iron produced by this method can meet the following standards: C≤0.002%, Si≤0.02%, Mn≤0.04%, P≤0.003%, S≤0.004%, Alt≤0.03%, and purity <99.9%. However, this method has complex process, high pretreatment cost, and low purity. Summary of the invention

[0004] The object of the present invention is to provide a method for producing high-purity raw pure iron continuous casting large square billet BGPI99, which adopts ginseng iron + molten iron desulfurization pretreatment + converter smelting + LF furnace refining + RH vacuum treatment + large square billet continuous casting (350mm×470mm) to produce high-purity raw pure iron continuous casting large square billet BGPI99, which not only ensures that the raw pure iron has a higher purity, but also ensures the lowest production cost, and meets the production needs of high-purity raw pure iron.

[0005] In order to achieve the above invention purpose, the present invention provides a method for producing high-purity raw material pure iron continuous casting large square billet BGPI99, comprising the following steps: using ginseng iron + hot metal desulfurization pretreatment + converter smelting + LF furnace refining + RH vacuum treatment + large square billet continuous casting (nominal cross-sectional size 350mm×470mm). The method can effectively improve the purity of raw material pure iron to meet the user's use requirements.

[0006] The composition of the molten steel in the step is controlled to be C: ≤0.0020%, Si: ≤0.005%, Mn: ≤0.030%, P: ≤0.0030%, S: ≤0.0010%, Cr: ≤0.0080%, Mo: ≤0.01%, Als: ≤0.05%, Cu: 0.0050%, Ni: ≤0.0050%, O: ≤0.0020%, Ti: ≤0.0005%, Ca: ≤0.0002%, Pb: ≤0.002%, Sb: ≤0.001%, Sn: ≤0.001%, As: ≤0.001%, Bi: ≤0.001%, and the remainder is iron and unavoidable impurities.

[0007] The specific steps are as follows:

[0008] (1) Pretreatment of molten iron desulfurization

[0009] The ore produced by Bengang's own iron mines is used to smelt hot metal in blast furnaces. The hot metal has low content of "five harmful elements" (Pb: ≤0.002%, Sb: ≤0.001%, Sn: ≤0.001%, As: ≤0.001%, Bi: ≤0.001%), low P (≤0.080%), and low S (≤0.030%), and is known as "ginseng iron". The hot metal is pre-treated with passivated magnesium powder and calcium oxide powder for desulfurization, wherein the amount of magnesium powder added is: 0.01kg to 0.05kg of magnesium powder is added according to the amount of S removed by 0.001% per ton of iron, and the weight ratio of calcium oxide powder to magnesium powder is (2:1)-(5:1), preferably 3:1; ensure that S in the hot metal after desulfurization is ≤0.002%, and then slag is removed.

[0010] In step (1), the IR method is used to spray passivated magnesium powder and calcium oxide powder to perform desulfurization pretreatment on the molten iron.

[0011] In step (1), the slag needs to be removed cleanly, and the amount of slag is ≤0.1t.

[0012] (2) Converter smelting

[0013] Using molten iron and thin plate low-sulfur (S≤0.003%) scrap steel for smelting, using double slag method for dephosphorization and demanganese operation, wherein the mass fraction of thin plate low-sulfur scrap steel accounts for 10-15% of the total amount of molten iron and thin plate low-sulfur scrap steel;

[0014] The first slag blowing process is to add active lime, limestone, magnesite, iron phosphorus balls, and oxygen supply, and then the first furnace slag discharge is carried out; after the slag discharge, the second slag blowing process is carried out, active lime is added, and oxygen is supplied for the second time. After the second oxygen blowing is completed, the spot blowing is carried out after calming for 2 to 5 minutes, and the spot blowing time is 40 to 60 seconds. The final oxygen of the converter is ≤800ppm, the final C is ≤0.04%, Mn is ≤0.05%, P is ≤0.008%, and S is ≤0.0025%. The slag is blocked for tapping, slag is strictly prohibited, and deoxidation is not performed. The tapping temperature is above 1650℃.

[0015] Among them, in the first slag making process, the amount of active lime added is 8-15kg / t steel, the amount of limestone added is 4-8kg / t steel, the amount of magnesite added is 5-10kg / t steel, the amount of iron phosphorus ball added is 4-8kg / t steel, the oxygen supply time is 4-6min, and the oxygen flow rate is 35000-40000Nm 3 / h; in the secondary slag making process, the amount of active lime added is 15-25kg / t steel, the oxygen supply time is 8-15min, and the oxygen flow rate is 35000-40000Nm 3 / h;

[0016] In step (2), a double-blown converter is used for production, and the amount of slag discharged for the first time is greater than 2 / 3.

[0017] (3) LF refining

[0018] The LF furnace uses the "double slag method" to remove Mn, P and S from the molten steel.

[0019] In the first slag making, active lime and iron phosphorus balls are added, the temperature is raised to 1620-1640℃, and Mn and P are removed from the slag at the same time, with the goal of removing Mn to less than 0.03% and P to less than 0.003%. After dephosphorization and demanganese removal, the oxidized slag is removed by "slag scooping" to prevent the return of Mn and P during the secondary slag making. The secondary slag making is mainly for S removal, active lime is added, and 100-200m of aluminum wire is fed to each furnace, and 100-150kg of aluminum particles are added to each furnace for precipitation deoxidation to make white slag by diffusion deoxidation, S is removed to less than 0.001%, and Mn / S is controlled to be greater than or equal to 5.

[0020] In the first slag making process, the amount of active lime added is 6-10kg / t steel, and the amount of iron-phosphorus balls added is 3-5kg / t steel; in the second slag making process, the amount of active lime added is 6-10kg / t steel;

[0021] (4) RH refining

[0022] The temperature of molten steel entering the RH furnace is 1590~1600℃. The RH adopts the forced decarburization mode. After the pump is turned on, the vacuum degree reaches below 1kPa for oxygen replenishment operation. The oxygen replenishment amount for each furnace is 100~200Nm 3, ensure that the oxygen content at the end of decarburization is not less than 300ppm, and the carbon at the end of RH is ≤0.0020%. After decarburization, deoxidation is carried out according to the oxygen content in the steel, but the oxygen content before RH leaving the station must be 20-60ppm, and the net circulation after deoxidation is not less than 10min. After re-pressing, add top slag modifier (30-50kg per furnace for cutting aluminum), and soft blow for more than 15min, with an argon flow rate of 80-120NL / min, to ensure that the deoxidation product fully floats.

[0023] (5) Continuous casting

[0024] A rectangular billet continuous casting machine is used for casting, and the molten steel is continuously cast into a large square billet BGPI99. The continuous casting is well protected. The tundish is purged with argon 10-15 minutes before pouring. Argon is passed through the tundish during the pouring process to ensure the reducing atmosphere of the tundish. A sealing ring should be used to seal the protective sleeve and the water outlet of the large ladle. The protective sleeve is prohibited from floating on the liquid surface during the pouring process. The tundish covering agent should be added evenly to ensure that the molten steel is not exposed to the liquid surface. The temperature of the first furnace of the large ladle is 1605-1615℃, the continuous casting is 1595-1605℃, the temperature of the tundish is 1555-1570℃, the pulling speed is 0.3-0.8m / min, the water volume of the second cooling water is 0.2-0.6L / kg steel, and the crystallizer is electromagnetically stirred.

[0025] In step (5), a 350 mm × 470 mm cross-section rectangular billet continuous casting machine is used for casting.

[0026] In step (5), carbon-free mold protection slag is used.

[0027] In step (5), the crystallizer electromagnetic stirring current is 200-500A, the end electromagnetic stirring current is 200-450A, and the frequency is 2-8Hz.

[0028] The advantage of the present invention is that in view of the purity of raw pure iron and the casting technology problems, by reasonably selecting the process route and reasonably designing the process parameters, a preparation method of high-purity raw pure iron continuous casting large square billet BGPI99 is provided, the purity of the steel is high and the residual element content is low; the Mn content can be controlled to within 0.03% and the P content can be controlled to within 0.003%, the surface quality of the billet is good, and the use requirements of raw pure iron customers at home and abroad are fully met. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Picture 1 This is a low-magnification inspection picture of the ingot. DETAILED DESCRIPTION

[0030] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0031] Example 1

[0032] A production method of high-purity raw material pure iron continuous casting large square billet BGPI99, the specific steps are as follows:

[0033] (1) Pretreatment of molten iron desulfurization

[0034] The iron ore produced by Bengang's own mines, smelted in blast furnaces, has the characteristics of low content of "five harmful elements" (Pb: ≤0.001%, Sb: ≤0.001%, Sn: ≤0.001%, As: ≤0.001%, Bi: ≤0.001%), low P (≤0.080%), and low S (≤0.030%), and is known as "ginseng iron". The IR method is used to spray passivated magnesium powder and calcium oxide powder to pre-treat the molten iron for desulfurization, in which the spraying amount of magnesium powder is: magnesium powder amount is 0.02kg / t steel, and the addition amount of calcium oxide powder is 0.05kg / t steel; the S content before treatment is 0.022%, and the S content in the molten iron after desulfurization is 0.002%, and the slag removal amount is 1.5t.

[0035] (2) Converter smelting

[0036] The smelting process is carried out by adding hot metal and thin plate low sulfur (S≤0.003%) scrap steel (the mass fraction of thin plate low sulfur scrap steel is 10%), using double blowing converter production, and using double slag method for dephosphorization and demanganese operation. The first slag making active lime addition amount is 11kg / t steel, limestone 5kg / t steel, magnesite 6kg / t steel, and iron phosphorus ball 5kg / t steel. Oxygen supply time 4min25s, oxygen flow rate 40000Nm 3 / h, the first furnace slag discharge is carried out, and the slag discharge volume is greater than 2 / 3; after the slag discharge, the secondary slag blowing is carried out, and the secondary slag is supplemented with 16.5kg / t steel of active lime, the secondary oxygen supply time is 9min30s, and the oxygen flow rate is 38000Nm 3 / h, after the secondary oxygen blowing is completed, the spot blowing is carried out after calming for 2 minutes, the spot blowing time is 48 seconds, the converter end oxygen is 580ppm, the end C: 0.02%, Mn: 0.048%, P: 0.007%, S: 0.010%. Slag blocking steel tapping, slag is strictly prohibited, no deoxidation, steel tapping temperature is above 1655℃.

[0037] (3) LF refining

[0038] The LF furnace adopts the "double slag method" for refining. First, 7kg / t of active lime and 4kg / t of iron phosphorus balls are added, and the temperature is raised to 1625℃ to slag and remove Mn and P. Mn is removed to 0.022% and P is removed to 0.002%. At the same time, the "slag scooping" method is used to remove the oxidized slag to prevent the return of Mn and P during the secondary slag making. For the secondary slag making and S removal, 300m of aluminum wire is first fed for precipitation deoxidation, and 6.5kg / t of active lime is added. The temperature is raised to 1610℃ to make slag, and white slag is made by diffusion deoxidation of aluminum particles. The total amount of aluminum particles added in each furnace is 128kg. After S removal, the sulfur content is 0.001%, Mn: 0.024%, and the Mn / S value is 24.

[0039] (4) RH refining

[0040] RH inlet temperature is 1595℃, RH adopts forced decarburization mode, after the pump is turned on for 8 minutes, the vacuum degree reaches below 1kPa and oxygen is added, the oxygen addition amount is 185Nm 3 , the oxygen content at the decarburization end point is 340ppm, and the carbon at the RH end point is 0.0012%. After decarburization, 108kg of aluminum particles are added for deoxidation, and the net circulation after deoxidation is 13min. After re-pressing, the top slag modifier (30kg of cutting aluminum per furnace) is added, and soft blowing is performed for 17min to ensure that the deoxidation product fully floats.

[0041] (5) Continuous casting

[0042] A 350mm×470mm cross-section rectangular billet continuous casting machine is used for casting. The continuous casting is well protected. The tundish is purged with argon 10 minutes before pouring. Argon is passed through the tundish during the pouring process to ensure the reducing atmosphere of the tundish. A sealing ring is used to seal the protective sleeve and the water outlet of the large ladle. The protective sleeve is prohibited from floating on the liquid surface during the pouring process. The tundish covering agent should be added evenly to ensure that the molten steel is not exposed to the liquid surface. The temperature of the first furnace of the large ladle is 1612℃, the temperature of the tundish is 1565℃, the pulling speed is 0.5m / min, the water volume of the second cooling water is 0.4L / kg steel, and carbon-free crystallizer protective slag is used. The crystallizer electromagnetic stirring current is 200A, the end electromagnetic stirring current is 240A, and the frequency is 8Hz.

[0043]

[0044] (6) Product quality

[0045] Chemical composition (mass percentage) / %

[0046] <![CDATA[ C ]]> <![CDATA[ S ]]> <![CDATA[ Mn ]]> <![CDATA[ P ]]> <![CDATA[ S ]]> <![CDATA[ Cr ]]> <![CDATA[ Als ]]> <![CDATA[ Mo ]]> <![CDATA[ Ni ]]> <![CDATA[ 0.0015 ]]> <![CDATA[ 0.001 ]]> <![CDATA[ 0.020 ]]> <![CDATA[ 0.0022 ]]> <![CDATA[ 0.0008 ]]> <![CDATA[ 0.007 ]]> <![CDATA[ 0.03 ]]> <![CDATA[ 0.001 ]]> <![CDATA[ 0.003 ]]> <![CDATA[ Cu ]]> <![CDATA[ Ti ]]> <![CDATA[ Sb ]]> <![CDATA[ Sn ]]> <![CDATA[ As ]]> <![CDATA[ Pb ]]> <![CDATA[ Bi ]]> <![CDATA[ O ]]> <![CDATA[ Ca ]]> <![CDATA[ 0.003 ]]> <![CDATA[ 0.0003 ]]> <![CDATA[ 0.001 ]]> <![CDATA[ 0.001 ]]> <![CDATA[ 0.001 ]]> <![CDATA[ 0.001 ]]> <![CDATA[ 0.001 ]]> <![CDATA[ 0.0015 ]]> <![CDATA[ 0.0001 ]]>

[0047] The surface quality of the ingot is good. The macrostructure of the ingot is dense and defect-free, with general porosity of 0.5 level, central porosity of 0.5 level, and ingot segregation of 0.5 level.

[0048] The ingot is rolled into rods, and the inclusions of categories A and B are all level 0.5, and those of categories C, D, and Ds are all level 0, with high purity.

Claims

1. A method for producing high-purity raw material pure iron continuous casting large square billet BGPI99, It is characterized in that The steps include: (1) Pretreatment of molten iron desulfurization The molten iron produced by smelting iron ore in a blast furnace is pre-treated with passivated magnesium powder and calcium oxide powder for desulfurization, wherein the amount of magnesium powder added is 0.01kg to 0.05kg based on the amount of S removed by 0.001% per ton of iron, and the weight ratio of the amount of calcium oxide powder to the amount of magnesium powder added is 2:1-5:1; ensure that the S in the molten iron after desulfurization is ≤0.002%, and then perform slag removal; (2) Converter smelting The molten iron and thin plate low-sulfur scrap steel are used for smelting after desulfurization pretreatment, and the double slag method is used for dephosphorization and demanganese operation; The first slag making and blowing, adding active lime, limestone, magnesite, iron phosphorus balls, oxygen supply, and then the first furnace pouring and slag discharge; after slag discharge, the second slag making and blowing, adding active lime, secondary oxygen supply, after the second oxygen blowing, calming for 2 to 5 minutes and then spot blowing, the spot blowing time is 40 to 60 seconds, the converter end oxygen ≤ 800ppm, the end C ≤ 0.04%, Mn ≤ 0.05%, P ≤ 0.008%, S ≤ 0.0025%, the tapping temperature is above 1650℃; Among them, in the first slag-making process, the amount of active lime added is 8-15kg / t steel, the amount of limestone added is 4-8kg / t steel, the amount of magnesite added is 5-10kg / t steel, the amount of iron phosphorus balls added is 4-8kg / t steel, and the oxygen supply time is 4-6min; in the secondary slag-making process, the amount of active lime added is 15-25kg / t steel, and the oxygen supply time is 8-15min; (3) LF refining The "double slag method" is used to remove Mn, P and S from molten steel. In the first slag making, active lime and iron phosphorus balls are added, and the temperature is increased to make slag, and Mn is removed to less than 0.03%, and P is removed to less than 0.003%. After dephosphorization and demanganization, the oxidized slag is removed, and then the secondary slag making is carried out, active lime is added, and white slag is made by using aluminum wire precipitation deoxidation and aluminum particle diffusion deoxidation to remove S to less than 0.001%, and Mn / S is controlled to be greater than or equal to 5; In the first slag making process, the amount of active lime added is 6-10kg / t steel, and the amount of iron-phosphorus balls added is 3-5kg / t steel; in the second slag making process, the amount of active lime added is 6-10kg / t steel; (4) RH refining The temperature of molten steel entering the RH furnace is 1590~1600℃, and the forced decarburization mode is adopted. After the pump is turned on, the vacuum degree reaches below 1kPa and oxygen is added. The oxygen addition amount is 100~200Nm 3 , ensure that the oxygen content at the end of decarburization is not less than 300ppm, and the end carbon is ≤0.0020%; after decarburization, deoxidation is carried out to ensure that the oxygen content is 20-60ppm, and the net circulation after deoxidation is not less than 10min, and the top slag modifier is added after re-pressurization, and soft blowing is carried out for more than 15min; (5) Continuous casting Continuously casting the molten steel into large square billets BGPI99; the size of the continuous casting large square billets is 350mm×470mm; Among them, the temperature of the first furnace of the large ladle is 1605-1615℃, the continuous casting is 1595-1605℃, the temperature of the tundish is 1555-1570℃, the casting speed is 0.5m / min, the water volume of the secondary cooling water is 0.4L / kg steel, and the crystallizer is electromagnetically stirred; The composition of the molten steel is as follows by mass percentage: C: ≤0.0020%, Si: ≤0.005%, Mn: ≤0.030%, P: ≤0.0030%, S: ≤0.0010%, Cr: ≤0.0080%, Mo: ≤0.01%, Als: ≤0.05%, Cu: 0.0050%, Ni: ≤0.0050%, O: ≤0.0020%, Ti: ≤0.0005%, Ca: ≤0.0002%, Pb: ≤0.002%, Sb: ≤0.001%, Sn: ≤0.001%, As: ≤0.001%, Bi: ≤0.001%, and the balance is iron and unavoidable impurities.

2. The production method according to claim 1, It is characterized in that In step (1), the IR method is used to spray passivated magnesium powder and calcium oxide powder to perform desulfurization pretreatment on the molten iron.

3. The production method according to claim 1, It is characterized in that In step (1), the slag needs to be removed cleanly, and the amount of slag is ≤0.1t.

4. The production method according to claim 1, It is characterized in that In step (2), the mass fraction of the thin plate low-sulfur scrap steel in the total amount of molten iron and the thin plate low-sulfur scrap steel is 10-15%.

5. The production method according to claim 1, It is characterized in that In step (2), a double-blown converter is used for production, and the amount of slag discharged for the first time is greater than 2 / 3.

6. The production method according to claim 1, It is characterized in that In step (4), the slag modifier is cutting aluminum, and the amount of cutting aluminum added is 30 to 50 kg per furnace.

7. The production method according to claim 1, It is characterized in that In step (5), a rectangular billet continuous casting machine is used for casting.

Citation Information

Patent Citations

  • A method for producing pure iron

    CN108277316B

  • High-cleanliness welding wire steel L-S3 and preparation method thereof

    CN114318154A

  • Non-aluminum deoxidation raw material pure iron for amorphous soft magnetic ribbon and preparation method of non-aluminum deoxidation raw material pure iron