Application of a surface modifier in carbon fiber modification
By using surface modifiers of lipophilic and hydrophilic groups with carbon fiber surface treatment, combined with semi-Diels-Alder reaction, the interfacial performance problems caused by inertness in the carbon fiber are solved, significantly improving its mechanical properties and reducing treatment costs and environmental impact.
Patent Information
- Application Number
- CN202310423438.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-19
AI Technical Summary
The inertness of the carbon fiber surface leads to poor interfacial performance when it is combined with other matrix materials. Existing surface treatment methods usually require high temperature and strong oxidation conditions, damage carbon fibers and waste resources, affecting their mechanical properties.
Using a surface modifier containing lipophilic groups and hydrophilic groups, it is prepared by semi-Diels-Alder reaction with compounds with C=C bonds or C≡C bonds and alkylene oxides, alkanes, olefins, and maleic anhydrides. Used for surface modification of carbon fibers to improve its mechanical properties.
The mechanical properties of carbon fiber are significantly improved, especially the mechanical properties of composite materials after being composited with other matrix materials. The processing process is low-carbon, energy-saving and environmentally friendly, avoiding damage to carbon fiber and waste of resources.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fine chemicals and organic synthesis, and more specifically, to the application of a surface modifier in carbon fiber modification. Background Art
[0002] Carbon fiber has excellent performance. It is not only light in weight, high in specific strength and modulus, but also resistant to corrosion by concentrated hydrochloric acid, phosphoric acid, sulfuric acid, benzene, acetone and other media, but also has high heat resistance and good chemical stability. The main uses of carbon fiber include being used as a reinforcing material, compounding with a resin matrix, preparing high-performance composite materials, and replacing traditional steel and other materials in the fields of energy, automobiles, oceans, aerospace, sports equipment, wind turbine blades, etc. Due to the inertness of the carbon fiber surface, it is difficult to compound with other matrix materials to prepare composite materials with good interface performance, which greatly limits the performance of its excellent performance. For this reason, it is necessary to treat the surface of the carbon fiber to improve its surface activity. At present, the commonly used surface treatment methods of carbon fiber are mainly dry and wet oxidation treatment of the carbon fiber surface, plasma treatment, electrochemical oxidation and surface chemical grafting. However, when these methods treat carbon fiber, they are usually accompanied by conditions such as high temperature and strong oxidation, which not only wastes a lot of energy and resources, but also often damages the carbon fiber and reduces its own mechanical properties. Therefore, it is of great practical significance to find a low-carbon, energy-saving and environmentally friendly treatment method that does not cause damage to the carbon fiber and affect its mechanical properties. Summary of the invention
[0003] Based on the above problems, the purpose of the present invention is to provide an application of a surface modifier in carbon fiber modification. In this application, the mechanical properties of the carbon fiber treated with the surface modifier are significantly improved, and the mechanical properties of the composite material prepared using the modified carbon fiber can be further improved.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] A surface modifier is used in carbon fiber modification, wherein the molecular structure of the surface modifier comprises a lipophilic group and a hydrophilic group; wherein:
[0006] The lipophilic group contains at least one functional group, and the functional group is selected from one or more of -H, alkyl, alkenyl, phenyl, aryl, cycloalkyl, cycloalkenyl and C≡C;
[0007] The hydrophilic group contains at least one functional group, and the functional group is selected from one or more of -H, -OH, alkoxy, aryl, aldehyde, carboxyl, ester, amino, cyano, nitro, halide, anhydride, sulfoxide, epoxy, sulfonyl, sulfonamide, sulfamoyl and carbamoyl.
[0008] Preferably, the carbon fiber modification includes improving the mechanical properties of the carbon fiber; more preferably, the mechanical properties include but are not limited to at least one of impact strength, tensile properties and notched impact.
[0009] Among them, the interface performance of the carbon fiber treated with the amphiphilic surface modifier is not only significantly improved, but the present invention also unexpectedly found that the mechanical properties of the modified carbon fiber are significantly improved, especially after being composited with other matrix materials, the mechanical properties of the composite material are more significantly improved.
[0010] Preferably, the surface modifier is obtained by a semi-Diels-Alder reaction between a compound containing a C=C bond or a C≡C bond and an alkylene oxide, an alkane, an alkene, or maleic anhydride. It is understood that this refers to a semi-Diels-Alder reaction between a compound containing a C=C bond or a C≡C bond and any one of the alkylene oxide, an alkane, an alkene, or maleic anhydride.
[0011] Preferably, the compound containing a C=C bond is selected from unsaturated fatty acids, olefins or maleic anhydride.
[0012] Preferably, the olefin is selected from C5-C30 olefins.
[0013] Preferably, the olefin is selected from normal olefins or internal olefins.
[0014] Preferably, the internal olefin is selected from one or more of internal-hexene, internal-heptene, internal-octene, internal-nonene, internal-decene, internal-undecene, internal-dodecene, internal-tridecene, internal-tetradecene, internal-pentadecaene, internal-hexadecene, internal-heptadecaene, internal-octadecene, internal-nonadecaene and internal-eicosene.
[0015] Preferably, the normal olefin is selected from n-hexene.
[0016] Preferably, the unsaturated fatty acid is selected from oleic acid or cis-3-hexenoic acid.
[0017] Preferably, the compound comprising a C≡C bond is selected from n-hexyne.
[0018] Preferably, the alkylene oxide is selected from one or more of propylene oxide, butylene oxide and ethylene oxide.
[0019] Preferably, the alkane is selected from one or more of n-hexane, n-hexadecane, cyclohexane and n-dodecane.
[0020] Preferably, the olefin is selected from n-hexene or internal olefins.
[0021] Preferably, the molar ratio of the compound containing a C=C bond or a C≡C bond to the alkylene oxide, alkane, olefin, and maleic anhydride is 1:50 to 50:1; preferably 1:1 to 1:10, and more preferably 1:1 to 1:5. It can be understood that 1:50 to 50:1 here refers to the ratio of the two reactants, that is, 1 / 50 to 50.
[0022] Preferably, the reaction temperature is 150°C to 300°C, more preferably 200°C to 250°C; illustratively, the temperature of the thermal reaction includes but is not limited to 150°C-250°C, 150°C to 180°C, 180°C to 200°C, 200°C to 220°C, 220°C to 250°C, etc.
[0023] Preferably, in the reaction, after the temperature reaches 180°C, the temperature is raised to 200°C-250°C at a rate of 9°C-13°C per hour (preferably 10°C per hour).
[0024] Preferably, the reaction pressure is 100 kPa to 1000 kPa, more preferably 100 kPa to 200 kPa; illustratively, the reaction pressure includes but is not limited to 100 kPa to 200 kPa, 200 kPa to 400 kPa, 400 kPa to 600 kPa, 600 kPa to 800 kPa, and 800 kPa to 1000 kPa.
[0025] Preferably, the reaction time is 5 h to 20 h, more preferably 10 h to 20 h; exemplary reaction times include but are not limited to 5 h to 8 h, 8 h to 10 h, 10 h to 12 h, 12 h to 14 h, 14 h to 16 h, 16 h to 18 h, 18 h to 20 h, etc.
[0026] Preferably, the reaction is carried out under stirring conditions, and the stirring rate is 50-500 rpm, more preferably 150-300 rpm; illustratively, the stirring rate includes but is not limited to 50-150 rpm, 150-300 rpm, 300-400 rpm, 400-500 rpm, etc.
[0027] Preferably, the reaction is carried out under anaerobic conditions.
[0028] Preferably, the raw materials of the reaction further include an auxiliary agent, the auxiliary agent includes an effective ingredient, and the effective ingredient includes one or two of hydroquinone, potassium halide and methylhydroquinone; and / or
[0029] The active ingredient contains 2,6-di-tert-butyl-p-cresol;
[0030] The auxiliary agent can be well used in the preparation of the surface modifier for carbon fiber modification. The auxiliary agent has good catalytic activity for the preparation of the catalytic surface modifier, and the addition amount is small, the separation is simple, no toxic and harmful gases are generated, and no environmental pollution is caused; it has good temperature resistance, and the maximum tolerable temperature is 350°C; the auxiliary agent has good regeneration and reuse performance, and the number of times it can be reused in the generation reaction is more than 100 times. The purity of the surface modifier obtained by the present invention is not less than 99%, the reaction yield is more than 85%, and it has high production practicality.
[0031] Preferably, the catechol is selected from hydroquinone, catechol or resorcinol.
[0032] Preferably, the potassium halide is selected from potassium bromide or potassium iodide.
[0033] Preferably, the auxiliary agent further comprises a carrier, and the active ingredient is loaded on the carrier.
[0034] Preferably, the carrier is selected from one or more of alumina (eg, α-Al2O3 or γ-Al2O3), silica, alumina-silica, titania, zeolite, kaolinite, clay, activated carbon and silicon carbide.
[0035] Preferably, the active ingredient accounts for 0.1%-90% of the total weight of the auxiliary agent, preferably 0.1%-30%, more preferably 15%-25%.
[0036] Preferably, the auxiliary agent is solid or liquid. The auxiliary agent is preferably solid, and the solid microscopic surface is rough and has a larger specific surface area.
[0037] Preferably, the auxiliary agent has ≥5m 2 / g. More preferably, it has a BET surface area of ≥10m 2 / g BET surface area. Still more preferably, having 6m 2 / g-9m 2 / g BET surface area. BET surface area can be calculated by N2 physical adsorption analysis.
[0038] Preferably, the auxiliary agent has a pore volume of 0.1 ml / g-1.0 ml / g. More suitably, the auxiliary agent has a pore volume of 0.3 ml / g-0.8 ml / g. More suitably, the auxiliary agent has a pore volume of 0.3 ml / g-0.6 ml / g. The pore volume can be calculated using any suitable technique known in the art, such as, for example, the technique described in Fuel Processing Technology 135, 2015, 195-202.
[0039] Preferably, the molar ratio of the auxiliary agent to the total raw materials of the reaction is 1:10 to 1:1000, preferably 1:10 to 1:100.
[0040] Preferably, the carbon fiber refers to carbon fiber or carbon fiber fabric reinforced polymer composite material.
[0041] Preferably, in the carbon fiber fabric reinforced polymer composite material, the polymer is selected from one or more of polyethylene, polypropylene, polystyrene, polyvinyl chloride and polyethylene terephthalate (PET).
[0042] Preferably, the application comprises the following steps:
[0043] The surface modifier is mixed with carbon fiber and molded.
[0044] It can be understood that when the carbon fiber refers to a carbon fiber fabric reinforced polymer composite material, it also includes the step of composite-molding the molded carbon fiber with a polymer.
[0045] Preferably, the weight of the surface modifier is 0.1%-10% of the weight of the carbon fiber.
[0046] In the present invention, "internal olefin" refers to "olefin with C=C at the internal position of the molecule".
[0047] In addition, unless otherwise specified, any range described in the present invention includes the end value and any numerical value between the end values and any sub-range formed by the end value or any numerical value between the end values.
[0048] The beneficial effects of the present invention are as follows:
[0049] The surface modifier provided by the present invention has a small amount of addition in the process of carbon fiber surface modification, is simple to separate, does not generate toxic and harmful gases, and does not cause environmental pollution; and has good temperature resistance, and can withstand a maximum temperature of 350°C.
[0050] In the application provided by the present invention, a surface modifier with a specific structure is used for carbon fiber modification for the first time, which effectively improves the mechanical properties of the carbon fiber, especially the tensile properties.
[0051] The carbon fiber modified with the surface modifier of the present invention can be used in carbon fiber fabric reinforced polymer composite materials to better improve their relevant mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0053] Figure 1 The UV-visible absorption spectrum of the surface modifier in Example 1 is shown.
[0054] Figure 2 The infrared absorption spectrum of the surface modifier in Example 1 is shown.
[0055] Figure 3 The appearance of the surface modifier additive prepared in Example 1 is shown. DETAILED DESCRIPTION
[0056] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0057] Some of the following embodiments include using olefins and alkylene oxides as raw materials, adding auxiliary agents, and synthesizing the target product surface modifier efficiently and selectively, and the specific reaction formula is:
[0058]
[0059] Wherein, in the above formula, R1 and R2 are straight-chain or branched alkyl groups, and the sum of the number of carbon atoms of R1 and R2 is 6-50.
[0060] The preparation of the surface modifier comprises the following steps: uniformly mixing mixed olefins and ethylene oxide, wherein the ethylene oxide and the olefins are mixed in a molar ratio of 1:1 to 4:1; then adding an auxiliary agent, wherein the ratio of the auxiliary agent to the total reactant is 1:10 to 1000; continuously stirring and heating, and rapidly heating to 180°C; then performing a catalytic reaction between 180°C and 250°C, and continuing for 10 to 20 hours; after the reaction is completed, filtering out the auxiliary agent, performing reduced pressure distillation on the solution, removing excess olefins (recovered for repeated use), and obtaining the surface modifier.
[0061] Some of the following embodiments include using olefins and maleic anhydride as raw materials, adding auxiliary agents, and synthesizing the target product with high efficiency and selectivity. The specific reaction formula is:
[0062]
[0063] Wherein, in the above formula, R1 and R2 are straight-chain or branched alkyl groups, and the sum of the number of carbon atoms of R1 and R2 is 6-50.
[0064] The preparation of the surface modifier comprises the following steps: uniformly mixing mixed olefins and maleic anhydride, wherein the maleic anhydride and the olefins are mixed in a molar ratio of 1:1-4; then adding an auxiliary agent, wherein the ratio of the auxiliary agent to the total reactant is 1:10-1000; continuously stirring and heating, and rapidly heating to 180°C; then performing a catalytic reaction between 180°C and 250°C, and continuing for 10-20 hours; after the reaction is completed, filtering out the auxiliary agent, performing reduced pressure distillation on the solution, removing excess olefins (recovered for repeated use), and obtaining the surface modifier.
[0065] Some of the following embodiments include using alkanes and maleic anhydride as raw materials, adding auxiliary agents, and synthesizing the target product with high efficiency and selectivity. The specific reaction formula is:
[0066] Wherein, in the above formula, R1 and R2 are straight-chain or branched alkyl groups, and the sum of the number of carbon atoms of R1 and R2 is 6-50.
[0067]
[0068] The preparation of the surface modifier comprises the following steps: uniformly mixing mixed alkanes and maleic anhydride, wherein the maleic anhydride and the alkanes are mixed in a molar ratio of 1:1-4; then adding an auxiliary agent, wherein the ratio of the auxiliary agent to the total reactant is 1:10-1000; continuously stirring and heating, and rapidly heating to 180°C; then performing a catalytic reaction at 180°C-250°C for 10-20 hours; after the reaction is completed, filtering out the auxiliary agent, performing reduced pressure distillation on the solution, removing excess alkanes (recovered for repeated use), and obtaining the surface modifier.
[0069] Example 1
[0070] A method for preparing a surface modifier comprises the following steps:
[0071] 40g cyclohexene, 15.3g propylene oxide and 1.90g 2,6-di-tert-butyl-p-cresol loaded on silica were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180℃, and then increased to 220℃ at a rate of 10℃ per hour, and the reaction was continued for 16h to obtain the desired surface modifier. After the auxiliary agent was recycled 20 times, the cyclohexene conversion rate reached 88%. The color of the obtained surface modifier is light yellow. The product structure is:
[0072]
[0073] Figure 1 The UV-visible absorption spectrum of the surface modifier in this example is shown. Figure 2 The infrared absorption spectrum of the surface modifier in this example is shown.-1 The stretching vibration peaks of methyl CH are on the left and right, 2800 cm -1 The CH stretching vibration peak of methylene is around 1900 cm -1 The stretching vibration peak of C=O is around 1800cm -1 is the stretching vibration peak of C=C, 1500cm -1 is the CH bending vibration peak, 1100cm -1 is the stretching vibration peak of CO, 900 cm -1 Nearby is the stretching vibration peak of =CH. Figure 3 The following is a diagram showing the appearance of the surface modifier prepared in this example.
[0074] Example 2
[0075] A method for preparing a surface modifier comprises the following steps:
[0076] 40g of n-hexene, 15.3g of cis-3-hexenol and 0.95g of 2,6-di-tert-butyl-p-cresol were weighed and added to the reactor to mix thoroughly. Nitrogen was introduced to exhaust the air. The system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180℃, and then increased to 220℃ at a rate of 10℃ per hour. The reaction was continued for 16h to obtain a surface modifier. The additive was recycled 20 times, and the conversion rate of n-hexene reached 82%. The color of the obtained surface modifier was light yellow. The product structure is:
[0077]
[0078] Example 3
[0079] A method for preparing a surface modifier comprises the following steps:
[0080] 40g of n-hexadecene, 15.3g of butylene oxide and 3.80g of 2,6-di-tert-butyl-p-cresol loaded on titanium dioxide were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180℃, and then increased to 220℃ at a rate of 10℃ per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of n-hexadecene reached 84%. The color of the obtained surface modifier is light yellow. The product structure is:
[0081]
[0082] Example 4
[0083] A method for preparing a surface modifier comprises the following steps:
[0084] 40g of dodecene, 15.3g of ethylene oxide and 1.90g of hydroquinone were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 100kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of dodecene reached 80%. The color of the obtained surface modifier is light yellow. The product structure is:
[0085]
[0086] Example 5
[0087] A method for preparing a surface modifier comprises the following steps:
[0088] 40g of octadecene, 15.3g of maleic anhydride and 1.90g of hydroquinone loaded on alumina were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 300kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of octadecene reached 85%. The color of the obtained surface modifier is brownish yellow. The product structure is:
[0089]
[0090] Example 6
[0091] A method for preparing a surface modifier comprises the following steps:
[0092] 40g of n-hexane, 15.3g of oleic acid and 1.90g of hydroquinone were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 100r / min, the temperature was gradually increased to 180℃, and then increased to 220℃ at a rate of 10℃ per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of n-hexane reached 78%. The color of the obtained surface modifier is brown-yellow. The product structure is:
[0093]
[0094] Example 7
[0095] A method for preparing a surface modifier comprises the following steps:
[0096] 40g of n-hexadecane, 15.3g of maleic anhydride and 1.90g of hydroquinone were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 300r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of n-hexadecane reached 83%. The color of the obtained surface modifier is brown-yellow. The product structure is:
[0097]
[0098] Example 8
[0099] A method for preparing a surface modifier comprises the following steps:
[0100] 40g cyclohexane, 15.3g oleic acid and 1.90g resorcinol loaded on alumina were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180℃, and then increased to 220℃ at a rate of 8℃ per hour, and the reaction was continued for 16h to obtain a surface modifier. After 20 cycles, the cyclohexane conversion rate reached 88%. The color of the obtained surface modifier is brown-yellow. The product structure is:
[0101]
[0102] Example 9
[0103] A method for preparing a surface modifier comprises the following steps:
[0104] 40g of n-hexyne, 15.3g of oleic acid and 1.90g of 2,6-di-tert-butyl-p-cresol supported on silica were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180℃, and then increased to 220℃ at a rate of 12℃ per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of n-hexyne reached 86%. The color of the obtained surface modifier is brown-yellow. The product structure is:
[0105]
[0106] Example 10
[0107] A method for preparing a surface modifier comprises the following steps:
[0108] 40g of n-eicosane, 15.3g of maleic anhydride and 1.90g of 2,6-di-tert-butyl-p-cresol were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 210°C at a rate of 10°C per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of n-eicosane reached 79%. The color of the obtained surface modifier is brown-yellow. The product structure is:
[0109]
[0110] Embodiment 11
[0111] A method for preparing a surface modifier comprises the following steps:
[0112] 20g of octadecene and 20g of hexadecene, 15.3g of cyclopropane and 1.90g of potassium bromide were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 230°C at a rate of 10°C per hour, and the reaction was continued for 16h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of octadecene and hexadecene reached 86%. The color of the obtained surface modifier is brown-yellow. The product structure is:
[0113] Among them, R1+R2=14.
[0114] Example 12
[0115] A method for preparing a surface modifier comprises the following steps:
[0116] 20g of inner dodecene and 20g of inner tetradecene were measured, 15.3g of maleic anhydride and 1.90g of catechol supported on alumina were weighed, all were added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 14h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of inner dodecene and inner tetradecene reached 86%. The color of the obtained surface modifier is brownish yellow. The product structure is:
[0117] Among them, R1+R2=8.
[0118] Embodiment 13
[0119] A method for preparing a surface modifier comprises the following steps:
[0120] 20g of hexadecene and 20g of octadecene were measured, 15.3g of maleic anhydride and 1.90g of catechol were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 14h to obtain a surface modifier. After the auxiliary agent was recycled 22 times, the conversion rate of hexadecene and octadecene reached 88%. The color of the obtained surface modifier is brownish yellow. The product structure is:
[0121] Among them, R1+R2=12.
[0122] Embodiment 14
[0123] A method for preparing a surface modifier comprises the following steps:
[0124] 20g of tetradecene and 20g of hexadecene were measured, 15.3g of maleic anhydride and 1.90g of catechol supported on titanium dioxide were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 14h to obtain a surface modifier. After the auxiliary agent was recycled for 25 times, the conversion rate of tetradecene and hexadecene reached 87%. The color of the obtained surface modifier is brownish yellow. The product structure is:
[0125] Among them, R1+R2=10.
[0126] Embodiment 15
[0127] A method for preparing a surface modifier comprises the following steps:
[0128] 20g of dodecene and 20g of octadecene were measured, 15.3g of maleic anhydride and 1.90g of catechol were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 14h to obtain a surface modifier. After the auxiliary agent was recycled 20 times, the conversion rate of dodecene and octadecene reached 86%. The color of the obtained surface modifier is brown-yellow. The product structure is:
[0129] Among them, R1+R2=8.
[0130] Example 16
[0131] A method for preparing a surface modifier comprises the following steps:
[0132] 20g of inner dodecene and 20g of inner tetradecene were measured, 15.3g of maleic anhydride and 1.90g of catechol were weighed, all added to the reactor and mixed thoroughly, nitrogen was introduced to exhaust the air, the system pressure was 200kPa, the stirring speed was set to 200r / min, the temperature was gradually increased to 180°C, and then increased to 220°C at a rate of 10°C per hour, and the reaction was continued for 14h to obtain a surface modifier. After the auxiliary agent was recycled 22 times, the conversion rate of inner dodecene and inner tetradecene reached 88%. The color of the obtained surface modifier is brownish yellow. The product structure is:
[0133] Among them, R1+R2=8.
[0134] Embodiment 17
[0135] Carbon fiber reinforcement test
[0136] The test method includes the following steps:
[0137] Preparation of samples modified with surface modifiers: Use 0.8 g of the surface modifier prepared in the above embodiments to surface treat 60 g of carbon fiber by an immersion pulling method or a coating method. Then put the surface-treated carbon fiber into an oven, heat the temperature to 70°C at a rate of 0.25-0.5°C / min and keep warm for 2 hours to obtain the modified carbon fiber. The reinforced carbon fiber materials prepared by the surface modifiers of Examples 1 to 16 are respectively recorded as Sample 1...Sample 16.
[0138] The mechanical properties of the samples were tested using the national standard (GB1040-79, plastic tensile test method) to test the tensile properties of the samples. The test results are shown in Table 1 below.
[0139] Table 1
[0140] sample Tensile properties(GPa) Unmodified 2.5 Sample 1 3.8 Sample 2 3.7 Sample 3 3.7 Sample 4 3.6 Sample 5 3.5 Sample 6 3.8 Sample 7 3.5 Sample 8 3.4 Sample 9 3.3 Sample 10 3.3 Sample 11 3.2 Sample 12 3.5 Sample 13 3.5 Sample 14 3.6 Sample 15 33 Sample 16 3.6
[0141] Embodiment 18
[0142] Carbon fiber and polypropylene composite testing
[0143] The test method includes the following steps:
[0144] Preparation of samples modified by surface modifier: 0.8g of surface modifier prepared in Examples 1 to 16 above was obtained respectively, and 60g of carbon fiber was subjected to surface modification by immersion and pulling method or coating method. Nine layers of carbon fiber and 10 layers of polypropylene film after surface modification were laid alternately, and then formed on a molding machine at 210°C to obtain a carbon fiber and polypropylene composite plate. They were respectively recorded as Sample 1…Sample 16.
[0145] Preparation of samples not modified by surface modifiers: 9 layers of carbon fiber and 10 layers of polypropylene film without surface modification were laid alternately, and then formed on a molding machine at 210°C to obtain a carbon fiber and polypropylene composite plate to obtain an unmodified sample.
[0146] The mechanical properties of the samples were tested using the national standard (GB1040-79, plastic tensile test method) to test the tensile properties of the samples. The test results are shown in Table 2 below.
[0147] Table 2
[0148] sample Tensile properties (MPa) Unmodified 210.4 Sample 1 550.8 Sample 2 540.2 Sample 3 530.4 Sample 4 530.8 Sample 5 521.5 Sample 6 549.8 Sample 7 540.3 Sample 8 530.5 Sample 9 520.4 Sample 10 534.8 Sample 11 520.9 Sample 12 530.8 Sample 13 520.6 Sample 14 550.4 Sample 15 532.5 Sample 16 524.6
[0149] Embodiment 19
[0150] Carbon fiber and polyethylene composite testing
[0151] The test method includes the following steps:
[0152] Preparation of samples modified by surface modifier: 0.8g of surface modifier prepared in Examples 1 to 16 was obtained respectively, and 60g of carbon fiber was subjected to surface modification by immersion and pulling method or coating method. Nine layers of carbon fiber and 10 layers of polyethylene film after surface modification were laid alternately, and then formed on a molding machine at 210°C to obtain a carbon fiber and polypropylene composite plate. They were respectively recorded as Sample 1…Sample 16.
[0153] Preparation of samples not modified by surface modifiers: 9 layers of carbon fiber and 10 layers of polypropylene film without surface modification were laid alternately, and then formed on a molding machine at 210°C to obtain a carbon fiber and polypropylene composite plate to obtain an unmodified sample.
[0154] The mechanical properties of the samples were tested using the national standard (GB1040-79, plastic tensile test method) to test the tensile properties of the samples. The test results are shown in Table 3 below.
[0155] Table 3
[0156]
[0157]
[0158] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. Application of a surface modifier in carbon fiber modification, characterized in that: The molecular structure of the surface modifier is shown below: 、 、 、 、 、 、 、 、 、 、 , Wherein, in the above formula, R1 and R2 are straight-chain alkyl groups, and the sum of the number of carbon atoms of R1 and R2 is 8, 12, 10 or 14.
2. The use according to claim 1, characterized in that: The carbon fiber modification is to improve the tensile properties of the carbon fiber.
3. The use according to claim 1 or 2, characterized in that: The carbon fiber refers to carbon fiber or carbon fiber fabric reinforced polymer composite material.
4. The use according to claim 3, characterized in that: In the carbon fiber fabric reinforced polymer composite material, the polymer is selected from one or more of polyethylene and polypropylene.
5. The use according to claim 3, characterized in that: The steps include: The surface modifier is mixed with carbon fiber and molded.
6. The use according to claim 5, characterized in that: The weight of the surface modifier is 0.1%-10% of the weight of the carbon fiber.
Citation Information
Patent Citations
Unsaturated epoxides as coupling agents for carbon fibers and unsaturated matrix resins
CA1082391A
Carbon fiber sizing agent and preparation method thereof, carbon fiber reinforced polypropylene composite material and preparation method of carbon fiber reinforced polypropylene composite material
CN107700213A
Polyester fiber, preparation method therefor, and tire cord comprising same
CN108431328A