Pigment for color filter, coloring composition, and color filter
By using a color filter coating composed of specific zinc halide phthalocyanine pigment and resin, the problem of taking into account both the color and brightness of the green pixel part under the BT2020 standard is solved, and the color filter with high brightness and film thickness is achieved, reducing the display's Consumption of power.
Patent Information
- Application Number
- CN202180069519.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-15
- Filing Date
- 2021-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-08-19
AI Technical Summary
It is difficult for existing color filters to achieve both high brightness and film thickness in the BT2020 color standard, especially around the chromaticity coordinates (x, y) = (0.170, 0.797) of the green pixel portion, and consumes high power.
Using zinc halide phthalocyanine pigment containing a specific number of halogen atoms, combined with appropriate resin composition and film thickness design, a green pixel coating film of the color filter is formed to show close to (x, y in the XYZ color system of CIE ) = (0.170, 0.797) chromaticity coordinates and increase brightness.
A color filter with thinner film thickness and excellent brightness in the BT2020 color standard is realized, reducing the power consumption requirement of the monitor.
Smart Images

Figure CN116323809B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a pigment for color filter, a coloring composition and a color filter. Background Art
[0002] In a display device such as a liquid crystal display device, the color of light from a light source is converted by a color filter having red, green, and blue color pixel portions to display an image. For such a display device, there are various standards related to color reproducibility, and it is required that the color can be displayed with a specified chromaticity corresponding to each standard. Therefore, the color filter used in the display device also needs to convert the light from the light source into light with a chromaticity corresponding to the standard.
[0003] The colorant for the green pixel portion in the color filter is required to have: (1) high brightness and (2) high color reproducibility.
[0004] In order to achieve (1) high brightness, it is important to select a pigment with a high transmittance to the backlight source, and Pigment Green 58 can be used as the main pigment. Current displays are designed to have high brightness under the sRGB standard (green pixel is (x, y) = (0.300, 0.600)), and LED-YAG is widely used as the backlight source. In order to achieve (2) high color reproduction, a pigment that can achieve vivid color display is required. It is proposed to use a green photosensitive resin composition containing Pigment Green 7 and Pigment Yellow 185 to form green pixels to achieve high color reproduction, but Pigment Green 7 has a low transmittance, so the brightness of the resulting display is low. As a new high color reproduction pigment, there is Pigment Green 59. If a comparison is made when making a color filter with the same film thickness, the brightness is higher when Pigment Green 59 is used than when Pigment Green 7 is used. In order to cover the standards of high color reproduction displays (Adobe RGB, DCI-P3, etc.), there is also a design that makes the film thickness of the color filter thicker, but there will be problems such as the inability to fully cure the color filter during the exposure process, so it is preferred to use a pigment that can achieve vivid color display. For the above reasons, Pigment Green 58 is used in a high-brightness display, and Pigment Green 59 is used in a high-color reproduction display. The color filters described above are described in, for example, Patent Documents 1 to 3 listed below.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2012-123302
[0008] Patent Document 2: Japanese Patent Application Publication No. 2006-045399
[0009] Patent Document 3: International Publication No. 2015 / 118720 Pamphlet Summary of the invention
[0010] Problems to be solved by the invention
[0011] In recent years, BT2020 has attracted attention as a color standard that is more vivid than the previous Adobe RGB and DCI-P3. In BT2020, the green pixel is designed with (x, y) = (0.170, 0.797) equivalent to the color light of 532nm, but it is understood that it is difficult to achieve such a pixel by using a color filter of pigment green 58 and 59 and a general light source. As the green pixel part of the color filter, it is necessary to allow light near 532nm to pass through and absorb light other than that. Although the development of light sources in recent years has been moving towards adjusting the maximum wavelength to near 532nm, unnecessary light will be included on the wavelength side shorter than 532nm and the wavelength side longer than 532nm, so it is necessary to combine appropriate color filters.
[0012] In order to make a green color filter corresponding to the new color standard BT2020, the problem is how to achieve chromaticity coordinates close to (x, y) = (0.170, 0.797) through a thin film. In addition, from the perspective of suppressing the power consumption of the display, the problem is also how to design a higher brightness at a chromaticity coordinate close to (x, y) = (0.170, 0.797).
[0013] Therefore, an object of the present invention is to provide a pigment that can be used to form a color filter having a thin film thickness of a green pixel portion and excellent brightness in accordance with BT2020, which is a new color standard.
[0014] Methods for solving problems
[0015] The inventors of the present invention have discovered that by using a zinc phthalocyanine halide pigment having a bluish (cyan) hue in a light source corresponding to BT2020 and having a specific number of halogen atoms, a chromaticity coordinate region close to (x, y) = (0.170, 0.797) can be displayed in the CIE XYZ color system, thereby solving the above-mentioned problem.
[0016] That is, the present invention is as follows.
[0017] Item 1. A color filter pigment, which is a pigment used for forming a coating film in a green pixel portion of a color filter,
[0018] When the film thickness of the coating film is set to 1.5 μm to 2.4 μm and the composition is set to 1.25 parts of resin per 1 part of the pigment in terms of mass conversion, in the XYZ colorimetric system of CIE when colorimetry is performed using only C light source, an xy chromaticity coordinate region surrounded by the following formulas (A) to (D) can be displayed:
[0019] Formula (A)
[0020] y=-1.766x+0.618
[0021] (where x is 0.10≤x≤0.17)
[0022] Formula (B)
[0023] y=5.889x-0.683
[0024] (where x is 0.15≤x≤0.17)
[0025] Formula (C)
[0026] y=0.125x+0.181
[0027] (where x is 0.07≤x≤0.15)
[0028] Formula (D)
[0029] y=8.380x-0.397
[0030] (where x is 0.07≤x≤0.10)
[0031] The above-mentioned pigment includes a compound represented by the following formula (1), namely a halogenated zinc phthalocyanine pigment, wherein the number of halogen atoms in one molecule of the above-mentioned compound is 0.2 or more and 10 or less on average, the number of bromine atoms in one molecule of the above-mentioned compound is 0.1 or more and 10 or less on average, and the number of chlorine atoms in one molecule of the above-mentioned compound is 0.1 or more and less than 2 on average.
[0032]
[0033] [In formula (1), X 1 ~X 16 Each independently represents a hydrogen atom or a halogen atom.]
[0034] Item 2. A colored composition comprising the pigment for color filter according to Item 1 and a solvent.
[0035] Item 3. A color filter comprising a coating film formed of the color filter pigment according to Item 1 in a green pixel portion.
[0036] Effects of the Invention
[0037] According to the pigment of the present invention, it is possible to provide a pigment having a thin film thickness in a green pixel portion and excellent brightness when formed into a color filter. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] [ Figure 1 ] is a diagram showing a color gamut close to BT2020 in the xy chromaticity diagram.
[0039] [ Figure 2 ] is a diagram showing an example of a spectrum of light from a light source.
[0040] [ Figure 3 ] is a diagram showing the pigment in the reference example using a monochromatic chromaticity diagram (x-axis: chromaticity x, y-axis: chromaticity y).
[0041] [Color filter pigments]
[0042] The pigment of the present invention is a pigment for forming a coating film in the green pixel portion of a color filter, and the pigment comprises a compound represented by the following formula (1), namely, a halogenated zinc phthalocyanine pigment, wherein the number of halogen atoms in one molecule of the compound is on average not less than 0.2 and not more than 10, the number of bromine atoms in one molecule of the compound is on average not less than 0.1 and not more than 10, and the number of chlorine atoms in one molecule of the compound is on average not less than 0.1 and less than 2.
[0043]
[0044] [In formula (1), X 1 ~X 16 Each independently represents a hydrogen atom or a halogen atom.]
[0045] Examples of the halogen atoms in the zinc phthalocyanine halogenide pigment of the compound represented by formula (1) include fluorine atoms, chlorine atoms, bromine atoms and iodine atoms. The average number of halogen atoms in one molecule is as described above, and the average number of bromine atoms and chlorine atoms in the zinc phthalocyanine halogenide pigment is as described above.
[0046] From the viewpoint of further improving the tinting power, the average number of halogen atoms in one molecule of the compound represented by formula (1) in the halogenated zinc phthalocyanine pigment is preferably 0.5 to 9.0, more preferably 1.0 to 7.0. From the viewpoint of obtaining a more excellent brightness, the average number of halogen atoms is preferably 2.0 to 9.0, more preferably 3.5 to 8.0.
[0047] From the viewpoint of obtaining better brightness and tinting power, the average number of bromine atoms in one molecule of the compound represented by formula (1) in the zinc phthalocyanine halide pigment is preferably 9.0 or less, and more preferably 6.5 or less. From the viewpoint of obtaining better brightness, the average number of bromine atoms is 0.1 or more, preferably 1.0 or more, and more preferably 2.0 or more.
[0048] From the viewpoint of obtaining better brightness and tinting power, the average number of chlorine atoms in one molecule of the compound represented by formula (1) in the zinc phthalocyanine halogenide pigment is preferably 1.9 or less, more preferably 1.6 or less, and further preferably 1.3 or less. From the viewpoint of obtaining better brightness, the average number of chlorine atoms is 0.1 or more, preferably 0.12 or more, more preferably 0.15 or more, and further preferably 0.2 or more.
[0049] The number of halogen atoms (e.g., the number of bromine atoms and the number of chlorine atoms) can be measured by fluorescent X-ray analysis. Specifically, the number of each halogen atom as a relative value per zinc atom can be calculated based on the mass ratio of zinc atoms to each halogen atom in the zinc phthalocyanine halide pigment.
[0050] The zinc phthalocyanine halogenide pigment is composed of one or more particles. The average particle size (average primary particle size) of the primary particles of the zinc phthalocyanine halogenide pigment may be 0.01 μm or more, 0.015 μm or more, or 0.02 μm or more. The average primary particle size of the zinc phthalocyanine halogenide pigment may be 0.20 μm or less, 0.10 μm or less, or 0.07 μm or less. Here, the average primary particle size is the average value of the major diameter of the primary particles, which can be obtained by measuring the major diameter of the primary particles in the same manner as the determination of the average aspect ratio described later.
[0051] The average aspect ratio of the primary particles of the zinc phthalocyanine halogenide pigment is, for example, 1.2 or more, 1.3 or more, 1.4 or more, or 1.5 or more. The average aspect ratio of the primary particles of the zinc phthalocyanine halogenide pigment is, for example, less than 2.0, 1.8 or less, 1.6 or less, or 1.4 or less. According to the zinc phthalocyanine halogenide pigment having such an average aspect ratio, a more excellent contrast can be obtained.
[0052] The zinc phthalocyanine halide pigment having an average aspect ratio of primary particles in the range of 1.0 to 3.0 preferably contains no primary particles having an aspect ratio of 5 or more, more preferably contains no primary particles having an aspect ratio of 4 or more, and further preferably contains no primary particles having an aspect ratio exceeding 3.
[0053] The aspect ratio and average aspect ratio of primary particles can be measured by the following method. First, the particles in the visual field are photographed by a transmission electron microscope (for example, JEM-2010 manufactured by JEOL Ltd.). Then, the longer diameter (major diameter) and the shorter diameter (minor diameter) of the primary particles present on the two-dimensional image are measured, and the ratio of the major diameter to the minor diameter is set to the aspect ratio of the primary particles. In addition, the average value of the major diameter and the minor diameter of 40 primary particles is obtained, and the ratio of the major diameter to the minor diameter is calculated using these values, which is set to the average aspect ratio. At this time, about the zinc phthalocyanine halogenide pigment as a sample, after making it ultrasonically dispersed in a solvent (for example, cyclohexane), it is photographed by a microscope. In addition, a scanning electron microscope can also be used to replace a transmission electron microscope.
[0054] The zinc phthalocyanine halide pigment of the present invention can be obtained through a step of synthesizing a crude pigment composed of at least a zinc phthalocyanine halide compound, and may further include a step of pigmenting the crude pigment as required.
[0055] The step of synthesizing the zinc phthalocyanine halide crude pigment may include a step of synthesizing the zinc phthalocyanine halide compound by a known production method such as a chlorosulfonic acid method, a phthalonitrile halide method, or a melting method.
[0056] The chlorosulfonic acid method includes a method in which zinc phthalocyanine is dissolved in a sulfur oxide solvent such as chlorosulfonic acid and chlorine gas or bromine is added thereto for halogenation. The reaction is carried out at a temperature of 20 to 120° C. for 3 to 20 hours.
[0057] As the halogenated phthalonitrile method, for example, the following method can be cited: phthalic acid or phthalonitrile after a part or all of the hydrogen atoms of the aromatic ring are replaced by halogen atoms such as bromine and chlorine, and zinc metal or zinc metal salt are appropriately used as starting materials to synthesize the corresponding halogenated zinc phthalocyanine compound. In this case, a catalyst such as ammonium molybdate can also be used as needed. The reaction at this time is carried out, for example, at a temperature of 100 to 300° C. and within a range of 7 to 35 hours.
[0058] As the melting method, the following method can be listed: zinc phthalocyanine is halogenated using a halogenating agent in a melt at about 10 to 170° C. consisting of one or a mixture of two or more of various compounds that serve as solvents during halogenation. The above-mentioned compounds are, for example, aluminum halides such as aluminum chloride and aluminum bromide, titanium halides such as titanium tetrachloride, alkali metal halides or alkaline earth metal halides (hereinafter referred to as alkaline (earth) metal halides) such as sodium chloride and sodium bromide, thionyl chloride, etc.
[0059] A preferred aluminum halide is aluminum chloride. In the above method using an aluminum halide, the amount of the aluminum halide added is usually 3 times or more, preferably 10 to 20 times the mole of zinc phthalocyanine.
[0060] Aluminum halide can be used alone, but if alkaline (earth) metal halide is used together with aluminum halide, the melting temperature can be further reduced, which is more advantageous in operation. The preferred alkaline (earth) metal halide is sodium chloride. Regarding the amount of alkaline (earth) metal halide added, within the range of generating a molten salt, the alkaline (earth) metal halide is preferably 1 to 15 parts by mass relative to 10 parts by mass of aluminum halide.
[0061] Examples of the halogenating agent include chlorine gas, sulfuryl chloride, and bromine.
[0062] The halogenation temperature is preferably 10 to 170° C., more preferably 30 to 140° C. In order to increase the reaction rate, pressure may be applied. The reaction time may be 5 to 100 hours, preferably 30 to 45 hours.
[0063] The melting method using two or more of the above compounds can arbitrarily control the content ratio of the zinc phthalocyanine compound composed of specific halogen atoms in the generated zinc phthalocyanine compound by adjusting the ratio of chloride, bromide and iodide in the molten salt, or changing the introduction amount of chlorine, bromine, iodine, etc. and the reaction time, so it is preferred. In addition, according to the melting method, the decomposition of the raw materials in the reaction is less and the yield from the raw materials is more excellent, and the reaction can be carried out by an inexpensive device without using a strong acid.
[0064] By optimizing the method of adding raw materials, the type of catalyst and its usage amount, the reaction temperature and the reaction time, a zinc phthalocyanine halide compound having a halogen atom composition different from that of the existing zinc phthalocyanine halide compound can be obtained.
[0065] Any of the above methods can be used after the reaction is completed, by dropping the obtained mixture into an acidic aqueous solution such as water or hydrochloric acid to precipitate the generated zinc phthalocyanine compound, thereby obtaining a zinc phthalocyanine halide crude pigment. As a zinc phthalocyanine halide crude pigment, it can be used directly, but it is preferably filtered, washed with water or sodium bisulfate water, sodium bicarbonate water, sodium hydroxide water, and then washed with an organic solvent such as acetone, toluene, methanol, ethanol, dimethylformamide as needed, and then used after post-treatment such as drying. The zinc phthalocyanine halide crude pigment can also be used after dry grinding in a pulverizer such as an attritor, a ball mill, a vibration mill, a vibration ball mill, etc. as needed.
[0066] The zinc phthalocyanine halide crude pigment obtained by the above process has the same composition as the zinc phthalocyanine halide pigment. The zinc phthalocyanine halide crude pigment obtained by the above process may be used as a pigment as it is, or may be further processed into a pigment as follows.
[0067] In the process of pigmenting the zinc phthalocyanine halogenide crude pigment, for example, the zinc phthalocyanine halogenide crude pigment is kneaded and ground to obtain the zinc phthalocyanine halogenide pigment. The process of pigmenting the zinc phthalocyanine halogenide crude pigment may also be a process of kneading the zinc phthalocyanine halogenide crude pigment with an inorganic salt and an organic solvent. Kneading may be performed using, for example, a kneader, a mixer, etc. In addition, the present invention may also include a process (a micronization process) of cooling the zinc phthalocyanine halogenide crude pigment to, for example, -50 to -10°C and grinding it together with a liquid organic solvent.
[0068] As the inorganic salt, a water-soluble inorganic salt can be preferably used. For example, inorganic salts such as sodium chloride, potassium chloride, and sodium sulfate are preferably used. The average particle size of the inorganic salt is preferably 0.5 to 50 μm. Such an inorganic salt can be easily obtained by finely pulverizing a common inorganic salt.
[0069] From the aspect of easily obtaining a pigment having an average primary particle size within the above range, it is preferred to make the amount of the inorganic salt used larger than the amount of the crude pigment used. Specifically, the amount of the inorganic salt used is preferably 5 to 20 parts by mass, more preferably 7 to 15 parts by mass, relative to 1 part by mass of the crude pigment.
[0070] The organic solvent may be an organic solvent that does not dissolve the crude pigment and the inorganic salt. As the organic solvent, it is preferred to use an organic solvent that can inhibit crystal growth. As such an organic solvent, it is preferred to use a water-soluble organic solvent. As the organic solvent, for example, diethylene glycol, glycerol, ethylene glycol, propylene glycol, liquid polyethylene glycol, liquid polypropylene glycol, 2-(methoxyethoxy)ethanol, 2-butoxyethanol, 2-(isopentyloxy)ethanol, 2-(hexyloxy)ethanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, trimethyl phosphate, 4-butyrolactone, propylene carbonate, N-methyl-2-pyrrolidone, methanol, ethylene cyanohydrin, 1,2,4-butanetriol, 1,2,5-pentanetriol, 1,3-butanediol, etc. can be used. The amount of the organic solvent (for example, a water-soluble organic solvent) used is not particularly limited, but is preferably 0.01 to 5 parts by mass based on 1 part by mass of the crude pigment.
[0071] From the viewpoint of preventing solidification due to cooling, the melting point of the organic solvent is preferably below -10°C, more preferably below -15°C, and further preferably below -20°C. The melting point of the organic solvent may be above -60°C. When the organic solvent contains a plurality of organic solvents, it is preferred that the melting point of at least one organic solvent is within the above range, and it is more preferred that the melting point of the entire organic solvent is within the above range.
[0072] From the viewpoint that the crude halogenated zinc phthalocyanine pigment is not easily dissolved and finer pigment particles are easily obtained, the organic solvent preferably contains an organic solvent having an Ra value of 5 or more with respect to zinc phthalocyanine. The Ra value represents the distance between the HSPs of two substances obtained from the dispersion force term (δd), polarity term (δp) and hydrogen bonding term (δh) in the Hansen Solubility Parameters (HSP). Since the dispersion force term (δd), polarity term (δp) and hydrogen bonding term (δh) of zinc phthalocyanine are 16.0, 7.7 and 9.5 respectively, if the dispersion force term of the organic solvent is set to δd1, the polarity term is set to δp1, and the hydrogen bonding term is set to δh1, the distance (Ra value) between the HSP of the organic solvent and the HSP of zinc phthalocyanine can be obtained by the following formula (I).
[0073] (Ra) 2 =4(δd1-16.0) 2 +(δp1-7.7) 2 +(δh1-9.5) 2 …(I)
[0074] Hansen solubility parameter values of various organic solvents are described in, for example, "Hansen Solubility Parameters: A Users Handbook" by Charles M. Hansen. Hansen solubility parameter values of organic solvents that are not described can be estimated using computer software (Hansen Solubility Parameters in Practice).
[0075] From the viewpoint of making the crude zinc phthalocyanine halogenide pigment less soluble, the Ra value of the organic solvent and zinc phthalocyanine is more preferably 10 or more. From the viewpoint of making the pigment easily wet, the Ra value of the organic solvent and zinc phthalocyanine is preferably 40 or less, more preferably 30 or less, and further preferably 25 or less.
[0076] When the organic solvent includes a plurality of organic solvents, the distance (Ra value) between the HSP of the organic solvent as a whole and the HSP of the zinc phthalocyanine halide calculated from the dispersion force term, polarity term and hydrogen bonding term of each organic solvent and the mixing ratio of each organic solvent is preferably within the above range.
[0077] In the micronizing step, water is preferably not used. The amount of water used is, for example, 20 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less, relative to 100 parts by mass of the crude zinc phthalocyanine halide pigment.
[0078] For cooling, for example, a cooling device such as a cooler (cooling water circulation device) can be used. When a cooler is used, the crude zinc phthalocyanine halogenide pigment can be cooled to about -50°C to -10°C by setting the temperature of the refrigerant in the cooler to, for example, -50°C to -10°C. From the viewpoint of obtaining finer pigment particles, the cooling temperature is preferably -20°C or less, more preferably -30°C or less. From the viewpoint of preventing an increase in the load on the grinding device due to high viscosity, the cooling temperature may exceed -50°C.
[0079] The grinding in the micronizing step can be performed using, for example, a kneader, a mixer, etc. The grinding time (for example, the kneading time) can be 1 to 60 hours.
[0080] When an inorganic salt and an organic solvent are used in the micronization process, a mixture containing a zinc phthalocyanine halide pigment, an inorganic salt and an organic solvent can be obtained. The organic solvent and the inorganic salt can be removed from the mixture, and the solid matter mainly containing the zinc phthalocyanine halide pigment can be washed, filtered, dried, pulverized, etc. as needed.
[0081] As washing, any of water washing and hot water washing can be adopted. Washing can be repeated within the range of 1 to 5 times. When a water-soluble inorganic salt and a water-soluble organic solvent are used, the organic solvent and the inorganic salt can be easily removed by washing with water. Acid washing, alkali washing, and organic solvent washing can also be performed as needed.
[0082] As the drying after the above-mentioned washing and filtration, for example, intermittent or continuous drying of the pigment for dehydration and / or desolvation by heating at 80 to 120° C. by a heating source provided in the dryer can be cited. As dryers, generally, box dryers, belt dryers, spray dryers, etc. can be cited. In particular, spray drying using a spray dryer is easy to disperse when making a slurry, so it is preferred. In addition, the pulverization after drying is not an operation for increasing the specific surface area or reducing the average particle size of the primary particles, but an operation for dispersing and powdering the pigment when the pigment is in a slope shape, such as when drying using a box dryer or a belt dryer. For example, pulverization by a mortar, a hammer mill, a disc mill, a pin mill, a jet mill, etc. can be cited.
[0083] In the above method, when the crude pigment is pigmented, the coating resin can be coexistent. By coexisting the resin during pigmentation, the active surface (active growth surface) of the particle is stabilized by the coated resin. Thus, the bias of the particle growth direction can be alleviated, so that a pigment with a small average aspect ratio can be easily obtained. By using such a pigment, the contrast of the pixel portion can be improved.
[0084] As the coating resin, it is preferred to use a resin having an acidic group, for example, a resin containing a polymer having an acidic group. Since the acidic group will show interaction with the active surface (active growth surface), by making the resin have an acidic group, a pigment with a small average aspect ratio of the primary particles can be easily obtained. As the acidic group, carboxyl, sulfonic acid, phosphoric acid and ammonium salt groups thereof can be listed. Among them, from the viewpoint of easily obtaining a more excellent contrast, a carboxyl group is preferred.
[0085] The pigment may further contain other components in addition to the above-mentioned zinc phthalocyanine halide pigment and the coating resin. Examples of other components include known phthalocyanine derivatives.
[0086] The zinc phthalocyanine halogenide pigment of the present invention has a unique cyan color. Compared with the conventional high-halogenide zinc phthalocyanine pigment, it has a bluish color instead of a yellowish color. It has specificity and can show a color that the conventional high-halogenide zinc phthalocyanine pigment cannot achieve.
[0087] In addition, when the zinc phthalocyanine halogenide pigment of the present invention is made into a coating film having a composition of 1.25 parts of resin per 1 part of pigment in terms of mass conversion and a film thickness of 1.5 μm to 2.4 μm, it can show an xy chromaticity coordinate area surrounded by the following formulas (A) to (D) in the XYZ colorimetric system of CIE when colorimetry is performed using only C light source.
[0088] Formula (A)
[0089] y=-1.766x+0.618
[0090] (where x is 0.10≤x≤0.17)
[0091] Formula (B)
[0092] y=5.889x-0.683
[0093] (where x is 0.15≤x≤0.17)
[0094] Formula (C)
[0095] y=0.125x+0.181
[0096] (where x is 0.07≤x≤0.15)
[0097] Formula (D)
[0098] y=8.380x-0.397
[0099] (where x is 0.07≤x≤0.10)
[0100] If the above equations (A), (B), (C), and (D) are shown in a chromaticity diagram (x-axis: chromaticity x, y-axis: chromaticity y), then Figure 3 The area enclosed by the formulas A, B, C, and D is the chromaticity coordinate area A.
[0101] In addition, from the perspective of excellent brightness when made into a color filter, the zinc phthalocyanine halogenide pigment of the present invention preferably exhibits an xy chromaticity coordinate region surrounded by the following formulas (C), (E), (F), and (G). When displayed on a chromaticity diagram, Figure 3 The area enclosed by the formulas C, E, F, and G is the chromaticity coordinate area B.
[0102] Formula (C)
[0103] y=0.125x+0.181
[0104] (where x is 0.07≤x≤0.15)
[0105] Formula (E): y = -1.333x + 0.503
[0106] (where x is 0.10≤x≤0.16)
[0107] Formula (F): y = 9.000x - 1.150
[0108] (where x is 0.15≤x≤0.16)
[0109] Formula (G): y = 6.000x - 0.230
[0110] (wherein x is 0.07≤x≤0.10).
[0111] Furthermore, from the perspective of excellent brightness when used as a color filter, the pigment of the present invention preferably exhibits an xy chromaticity coordinate region surrounded by the following formulas (E), (H), (I), and (J). When shown in a chromaticity diagram, Figure 3 The area enclosed by the formulas E, H, I, and J is the chromaticity coordinate area C.
[0112] Formula (E): y = -1.333x + 0.503
[0113] (where x is 0.10≤x≤0.16)
[0114] Formula (H): y = 7.000x - 0.830
[0115] (where x is 0.15≤x≤0.16)
[0116] Formula (I): y = -0.286x + 0.263
[0117] (where x is 0.08≤x≤0.15)
[0118] Formula (J): y = 6.500x - 0.280
[0119] (Wherein, x is 0.08≤x≤0.10).
[0120] The coating film is composed of 1.25 parts of resin per 1 part of pigment in terms of mass conversion. The resin is a resin for forming a coating film, preferably an acrylic resin, among which benzyl methacrylate-methacrylic acid copolymer and dimethylaminoethyl methacrylate copolymer are particularly preferred. As the benzyl methacrylate-methacrylic acid copolymer, for example, UNIDIC ZL-295 (solid content 40% by mass solution) manufactured by DIC Corporation can be used. The weight average molecular weight Mw of the benzyl methacrylate-methacrylic acid copolymer is, for example, 12000 to 16000. In addition, as the dimethylaminoethyl methacrylate copolymer, for example, BYK-LPN6919 (solid content 60% by mass solution) manufactured by BYK-Chemie can be used. The weight average molecular weight Mw of the dimethylaminoethyl methacrylate copolymer is, for example, 7000 to 11000. The dimethylaminoethyl methacrylate copolymer is, for example, a copolymer which provides a pigment dispersion having a viscosity of 10 mPa·s or less at 25° C. when 30 g of Pigment Green 58 (e.g. Fastogen Green A110 manufactured by DIC Corporation), 22.5 g of a resin solution containing 40% by mass of the above-mentioned benzyl methacrylate-methacrylic acid copolymer (e.g. ZL-295 manufactured by DIC Corporation), 132.5 g of propylene glycol monomethyl ether acetate, and 15 g of a resin solution containing 60% by mass of the above-mentioned dimethylaminoethyl methacrylate copolymer are dispersed for 2 hours using 460 g of 0.3 to 0.4 mm zirconium beads by a paint shaker to prepare a pigment dispersion. The above-mentioned viscosity is a viscosity measured by a cone-plate type rotational viscometer (cone-plate viscometer) (e.g. RE550L manufactured by Toki Sangyo Co., Ltd.) in accordance with JIS Z8803.
[0121] The above-mentioned coating film is not particularly limited and can be formed by the following method. First, using zirconium beads of 0.3 to 0.4 mm, 2.48 g of zinc phthalocyanine halogenide pigment is dispersed together with 1.24 g of BYK-LPN6919, 1.86 g of UNIDIC ZL-295 and 10.92 g of propylene glycol monomethyl ether acetate for 2 hours to prepare a pigment dispersion. 0.98 g of UNIDIC ZL-295 and 0.22 g of propylene glycol monomethyl ether acetate are added to 4.0 g of the obtained pigment dispersion, and mixed using a paint shaker to prepare a coating solution. Next, the coating solution is spin-coated on a soda glass substrate, dried at 90° C. for 3 minutes, and heated at 230° C. for 1 hour to form a coating film. The chromaticity is, for example, a value measured using a spectrophotometer (U-3900) manufactured by Hitachi High-Tech Industries, Ltd.
[0122] <Coloring Composition>
[0123] The coloring composition of the present invention contains at least the above-mentioned halogenated zinc phthalocyanine pigment and a solvent.
[0124] The coloring composition may further contain a resin that covers the zinc phthalocyanine halide pigment (covering resin). The type and content of the covering resin may be the same as those described as the covering resin contained in the above pigment composition, and the preferred embodiments are also the same.
[0125] As the solvent, an organic solvent is preferred. Examples of the organic solvent include aromatic solvents such as toluene, xylene, and methoxybenzene; acetate solvents such as ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; propionate solvents such as ethoxyethyl propionate; alcohol solvents such as methanol and ethanol; ether solvents such as butyl cellosolve, propylene glycol monomethyl ether, diethylene glycol ethyl ether, and diethylene glycol dimethyl ether; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aliphatic hydrocarbon solvents such as hexane; nitrogen compound solvents such as N,N-dimethylformamide, γ-butyrolactam, N-methyl-2-pyrrolidone, aniline, and pyridine; lactone solvents such as γ-butyrolactone; carbamates such as a mixture of methyl carbamate and ethyl carbamate in a ratio of 48:52, and the like. The organic solvent is preferably a polar solvent soluble in water, and more preferably a propionate solvent, an alcohol solvent, an ether solvent, a ketone solvent, a nitrogen compound solvent, or a lactone solvent.
[0126] The content of the solvent may be 300 parts by mass or more and 1000 parts by mass or less relative to 100 parts by mass of the total amount of the pigment.
[0127] As required, considering the economic efficiency, the coloring composition may further include organic pigments, organic dyes, organic pigment derivatives, etc. other than the halogenated zinc phthalocyanine pigment. As the organic pigment, the green halogenated copper phthalocyanine pigments, other green halogenated heterogeneous metal phthalocyanine pigments and the like, which are commonly known, can be used. In addition, yellow pigments for coloring can also be used. As yellow pigments, for example, yellow organic pigments such as CI Pigment Yellow 83, CI Pigment Yellow 110, CI Pigment Yellow 129, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 150, CI Pigment Yellow 180, CI Pigment Yellow 185, and CI Pigment Yellow 231 can be listed. Regarding the combined use ratio of the halogenated zinc phthalocyanine pigment and the yellow pigment, for example, the yellow pigment is 1 to 400 parts by mass relative to 100 parts by mass of the halogenated zinc phthalocyanine pigment. The organic pigment derivatives, for example, can be derivatives in which a part of the known organic pigment is modified (substituted) by sulfonic acid groups, carboxyl groups, amino groups, phthalimide methyl groups, etc. Specific examples include Solsperse (registered trademark) 5000, Solsperse 12000, and Solsperse 22000 (manufactured by The Lubrizol Corporation).
[0128] The coloring composition may further contain a dispersant as a component other than the above. As the dispersant, a known and commonly used dispersant such as a resin having an amine value can be used.Examples of the dispersant include ANTI-TERRA (registered trademark) U / U100, ANTI-TERRA 204, DISPERBYK (registered trademark) 106, DISPERBYK 108, DISPERBYK 109, DISPERBYK 112, DISPERBYK 130, DISPERBYK 140, DISPERBYK 142, DISPERBYK 145, DISPERBYK 161, DISPERBYK 162, DISPERBYK 163, DISPERBYK 164, DISPERBYK 167, DISPERBYK 168, DISPERBYK 180, DISPERBYK 182, DISPERBYK 183, DISPERBYK 184, DISPERBYK 185.DISPERBYK 2000,DISPERBYK 2001,DISPERBYK 2008,DISPERBYK 2009,DISPERBYK 2013,DISPERBYK 2022,DISPERBYK 2025,DISPERBYK 2026,DISPERBYK 2050,DISPERBYK 2055, DISPERBYK 2150, DISPERBYK 2155, DISPERBYK 2163, DISPERBYK 2164, DISPERBYK 9076, DISPERBYK 9077, BYK LPN-6919, BYK LPN-21116, BYK LPN-21324, BYK LPN-22102 (manufactured by BYK-Chemie Co., Ltd.), EFKA (registered trademark) 46, EFKA 47, EFKA 4010, EFKA 4020, EFKA 4320, EFKA 4300, EFKA 4330, EFKA 4401, EFKA 4570, EFKA 5054, EFKA 7461, EFKA 7462, EFKA7476, EFKA 7477 (manufactured by BASF Corporation), Ajisper (registered trademark) PB814, Ajisper PB821, Ajisper PB822, Ajisper PB881 (manufactured by Ajinomoto Fine-Techno Co., Ltd.), Solsperse (registered trademark) 24000, Solsperse 28000, Solsperse 37500, Solsperse 76500 (manufactured by Lubrizol Corporation), etc.The content of the dispersant may be 5 parts by mass or more and 120 parts by mass or less relative to 100 parts by mass of the total amount of the pigment.
[0129] The coloring composition may further contain a leveling agent, a coupling agent, a cationic rosin, a surfactant, a binder resin, a photosensitive compound (for example, a photosensitive resin), a curable resin, and the like as components other than the above.
[0130] A coloring composition containing a photosensitive compound may also be referred to as a photosensitive coloring composition. Examples of the photosensitive compound include thermoplastic resins such as polyurethane resins, acrylic resins, polyamic acid resins, polyimide resins, styrene maleic acid resins, and styrene maleic anhydride resins; bifunctional monomers such as 1,6-hexanediol diacrylate, ethylene glycol diacrylate, neopentyl glycol diacrylate, triethylene glycol diacrylate, bis(acryloyloxyethoxy)bisphenol A, and 3-methylpentanediol diacrylate; trimethylolpropane triacrylate, pentaerythritol triacrylate, tri(2-acryloyloxyethyl) isocyanurate, dipentaerythritol hexaacrylate, and dipentaerythritol pentaacrylate; and photopolymerizable monomers.
[0131] The photosensitive coloring composition may further contain a photopolymerization initiator. Examples of the photopolymerization initiator include acetophenone, benzophenone, benzyl dimethyl ketal, benzoyl peroxide, 2-chlorothioxanthone, 1,3-bis(4'-azidobenzylidene)-2-propane, 1,3-bis(4'-azidobenzylidene)-2-propane-2'-sulfonic acid, and 4,4'-bisazidostilbene-2,2'-disulfonic acid.
[0132] The method for producing the photosensitive coloring composition is not particularly limited, but is generally the following method: after preparing a dispersion (coloring composition) using a zinc phthalocyanine halogenide pigment or a pigment composition containing the zinc phthalocyanine halogenide pigment, a solvent, and a dispersant as required, a photosensitive compound is added thereto for preparation. In this case, the content of the photosensitive resin may be 3 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the above-mentioned dispersion. The content of the photopolymerization initiator may be 0.05 parts by mass or more and 3 parts by mass or less relative to 1 part by mass of the photosensitive resin.
[0133] In the case of using a yellow pigment for toning, for example, a dispersion liquid can be prepared by using a yellow pigment, a solvent and a dispersant as needed, and then a dispersion liquid containing a zinc phthalocyanine halide pigment, a dispersion liquid containing a yellow pigment and a photosensitive compound can be mixed to prepare a photosensitive coloring composition. In addition, a green toning composition can be prepared by adding a photosensitive compound to a dispersion liquid containing a zinc phthalocyanine halide pigment, a yellow toning composition can be prepared by adding a photosensitive compound to a dispersion liquid containing a yellow pigment, and the green toning composition can be mixed with the yellow toning composition to prepare a photosensitive coloring composition. As yellow pigments for toning, for example, CI Pigment Yellow 138, CI Pigment Yellow 185, CI Pigment Yellow 150, CI Pigment Yellow 129, CI Pigment Yellow 231 and CI Pigment Yellow 233 can be listed.
[0134] In the green pixel, the pigment ratio of the present invention is, for example, 10 to 90% by mass, preferably 20 to 80% by mass, relative to the total amount of the color material constituting the green pixel. In addition, the ratio of the yellow color material for color matching is, for example, 10 to 90% by mass, preferably 20 to 80% by mass, relative to the total amount of the color material constituting the green pixel.
[0135] <Color Filter>
[0136] The color filter of the present invention has a green pixel portion containing at least a zinc phthalocyanine halogenide pigment. In the color filter, the green pixel portion has a function of converting the color of the light from the light source. Usually, the color filter has a red pixel portion, a blue pixel portion and a shading portion (black matrix) in addition to the green pixel portion. In the color filter, the red pixel portion, the green pixel portion and the blue pixel portion are repeatedly configured in sequence, and the pixel portions of each color are separated from each other by the shading portion.
[0137] (light source)
[0138] An example of the spectrum of light from a light source is shown in Figure 2 . Figure 2 The spectrum in the wavelength region of 380 to 780 nm is shown. Figure 2 In the spectra shown, A.LED+QD and B.LED KSF are examples of the case where the light source is a white LED light source, which is a combination of a blue LED, a red light emitting phosphor, and a green light emitting phosphor, and obtains white light by mixing colors. It should be noted that the spectrum of light from the light source can be measured using a microscope MX-50 manufactured by Olympus and a spectrophotometer MCPD-3000 microscopic spectrophotometry device manufactured by Otsuka Electronics under the conditions of a measurement range of 380 to 780 nm and a measurement interval of 1 nm.
[0139] In the present invention, in the light emitted by the light source, the maximum wavelength in 480 to 580 nm is, for example, 500 to 560 nm, preferably 500 to 540 nm. A light source with a maximum wavelength in this range is preferred in BT2020 because the light of 510 to 532 nm is stronger. In addition, in the emitted light, the intensity (I480) of 480 nm is, for example, less than 1.1 relative to the intensity (I532) of 532 nm, preferably less than 1.0. In addition, the intensity (I480) of 480 nm is less than 0.9 relative to the intensity (I550) of 550 nm, preferably less than 0.8. By satisfying this intensity with light, the brightness in BT2020 can be improved.
[0140] In addition, in the present invention, the maximum wavelength of the light from the light source in the range of 480 to 580 nm is, for example, 500 to 560 nm, the intensity (I480) of 480 nm relative to the intensity (I532) of 532 nm is, for example, 1.1 or less, and the intensity (I480) of 480 nm relative to the intensity (I550) of 550 nm is 0.9 or less. Among them, the maximum wavelength of the light in the range of 480 to 580 nm is preferably 510 to 550 nm, the intensity (I480) of 480 nm relative to the intensity (I532) of 532 nm is 0.4 or less, and the intensity (I480) of 480 nm relative to the intensity (I550) of 550 nm is 0.4 or less. It is particularly preferred that the intensity of light at 480 nm (I480) is 0.2 or less relative to the intensity of light at 532 nm (I532), and the intensity of light at 480 nm (I480) is 0.2 or less relative to the intensity of light at 550 nm (I550).
[0141] As a light source emitting the above light, in addition to the above, for example, it can also be a white LED (light emitting diode) light source, a white organic EL light source, a white inorganic EL light source, a white quantum dot light source, etc. In the case where the light source is a white LED light source, the white LED light source can be listed as follows: a white LED light source that combines a red LED, a green LED, and a blue LED and obtains white light by mixing colors; a white LED light source that combines a blue LED, a red LED, and a green phosphor and obtains white light by mixing colors; a white LED light source that combines a blue LED, a red light-emitting phosphor, and a green light-emitting phosphor and obtains white light by mixing colors; a white LED light source that obtains white light by mixing colors of a blue LED and a YAG-based phosphor; a white LED light source that combines an ultraviolet LED, a red light-emitting phosphor, a green light-emitting phosphor, and a blue light-emitting phosphor and obtains white light by mixing colors; a white LED light source obtained by combining a red laser; a white LED light source obtained by using quantum dot technology, etc.
[0142] As a light source, Figure 2An example of a spectrum of the intensity of light of each wavelength is shown in FIG. As such a light source, commercially available products such as a green LED (e.g., model "NSPG336CS", manufactured by Nichia Chemical Industries, Ltd.), an LED KSF (e.g., model "NFSW157J-HG", manufactured by Nichia Chemical Industries, Ltd.), and an LED YAG1 (e.g., model "NSSW410A", manufactured by Nichia Chemical Industries, Ltd.) can be used.
[0143] When the color filter of the present invention uses the color material described later, it can display chromaticity coordinates close to BT2020 in the XYZ color system of CIE (International Commission on Illumination) when the above-mentioned light source is used for color measurement, that is, 0.140≤chromaticity x≤0.200, 0.600≤chromaticity y≤0.797. It should be noted that the XYZ color system is based on the mixing amount of the three primary colors of RGB (red / green / blue) color light, and is a concept usually used when considering the display color gamut in a display device.
[0144] The green pixel portion containing the zinc phthalocyanine halogenide pigment can be easily formed by the above-mentioned coloring composition (photosensitive coloring composition). As a specific method, for example, a method called photolithography can be cited, that is, by a spin coating method, a roller coating method, an inkjet method, etc., the coloring composition (photosensitive coloring composition) is applied to a transparent substrate such as a glass substrate, and then the coated film is exposed to ultraviolet light through a photomask, and then the unexposed portion is cleaned by an organic solvent, alkaline water, etc., thereby obtaining a coloring pattern. The method for forming the pixel portion is not particularly limited, for example, the pattern of the pixel portion can be formed by methods such as electrodeposition, transfer, micellar electrolysis, PVED (photovoltaic electrodeposition), etc., thereby manufacturing a color filter.
[0145] Other pixel portions (for example, a red pixel portion and a blue pixel portion) can also be formed by the same method using known pigments. Example
[0146] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to the following examples.
[0147] <Synthesis of Halogenated Zinc Phthalocyanine Pigments>
[0148] Halogenated zinc phthalocyanine pigments (RP1) to (RP4) were synthesized by the methods of the following Synthesis Examples 1 to 4. The average atomic number of halogen atoms in each pigment is shown in Table 1.
[0149] [Synthesis example 1]
[0150] 190 g of sulfonyl chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 315 g of aluminum chloride (manufactured by Kanto Chemical Co., Ltd.), 43 g of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), 84 g of zinc phthalocyanine (manufactured by DIC Corporation) and 185 g of bromine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 1L flask. The mixture was heated to 55°C, taken out into water, filtered, washed with water and dried to obtain zinc phthalocyanine halide (R1). 40 g of zinc phthalocyanine halide (R1), 400 g of crushed sodium chloride and 63 g of 1,3-butanediol (melting point: -54°C) were added to a double-arm kneader, and the cooling water circulation device was set to -20°C, and kneaded for 20 hours. The kneaded mixture was taken out into 2 kg of water at 80°C and stirred for 1 hour. Then, the mixture was filtered, washed with hot water, dried, and crushed to obtain a zinc phthalocyanine halogenide pigment (RP1) as a cyan pigment. The zinc phthalocyanine halogenide pigment (RP1) was subjected to fluorescent X-ray analysis using ZSX100E manufactured by Rigaku Corporation. The average number of chlorine atoms and the average number of bromine atoms were calculated based on the mass ratio of zinc atoms, chlorine atoms, and bromine atoms, as relative values per zinc atom. It should be noted that 1 g of the zinc phthalocyanine halogenide pigment was press-formed. The test specimen is made into a test piece. The measurement was performed in a vacuum atmosphere. As a result, in the zinc phthalocyanine halogenide pigment (RP1), the number of halogen atoms in one molecule was 8.1 on average, of which the number of bromine atoms was 7.9 on average and the number of chlorine atoms was 0.2 on average.
[0151] [Synthesis example 2]
[0152] A zinc phthalocyanine halogenide pigment (hereinafter also referred to as "zinc phthalocyanine halogenide pigment (RP2)") was prepared in the same manner as in Comparative Example 3 of Japanese Patent Application Laid-Open No. 2016-57635. The average number of chlorine atoms and the average number of bromine atoms of the zinc phthalocyanine halogenide pigment (RP2) were calculated in the same manner as in Synthesis Example 1. In the zinc phthalocyanine halogenide pigment (RP2), the average number of halogen atoms in one molecule was 10.0, of which the average number of bromine atoms was 6.9 and the average number of chlorine atoms was 3.1.
[0153] [Synthesis example 3]
[0154] A zinc phthalocyanine halogenide pigment (hereinafter also referred to as "zinc phthalocyanine halogenide pigment (RP3)") was prepared in the same manner as pigment 10 of manufacturing example 10 of Japanese Patent Publication No. 2018-36520. For the zinc phthalocyanine halogenide pigment (RP3), the average number of chlorine atoms and the average number of bromine atoms were calculated in the same manner as in Synthesis Example 1. In the zinc phthalocyanine halogenide pigment (RP3), the number of halogen atoms in one molecule is 7.3 on average, of which the number of bromine atoms is 2.0 on average and the number of chlorine atoms is 5.3 on average.
[0155] [Synthesis Example 4]
[0156] A zinc phthalocyanine halogenide pigment (hereinafter also referred to as "zinc phthalocyanine halogenide pigment (RP4)") was prepared in the same manner as RP4 of Example 4 of International Publication 2020 / 045199 (Japanese Patent Application 2020-520089). For the zinc phthalocyanine halogenide pigment (RP4), the average number of chlorine atoms and the average number of bromine atoms were calculated in the same manner as in Synthesis Example 1. In the zinc phthalocyanine halogenide pigment (RP4), the number of halogen atoms in one molecule is 10.4 on average, of which the number of bromine atoms is 9.3 on average and the number of chlorine atoms is 1.2 on average.
[0157] [Table 1]
[0158]
[0159] Next, cyan pigment dispersions (RMG1) to (RMG4), (SMG2) and a green pigment dispersion (SMG1) were prepared by the following method, an evaluation composition (RCG) and a coloring composition (TY) were further prepared, evaluation compositions (RDG), (SDG), (REG) and (SEG) were prepared and the color filter characteristics were evaluated.
[0160] <Example 1>
[0161] Using zirconium beads of 0.3 to 0.4 mm, 2.48 g of halogenated zinc phthalocyanine pigment (RP1) was dispersed together with 1.24 g of BYK LPN-6919 (manufactured by BYK-Chemie, trade name, solid content: 60 mass %), 1.86 g of UNIDIC ZL-295 (manufactured by DIC Corporation, trade name, solid content: 40 mass %) and 10.92 g of propylene glycol monomethyl ether acetate for 2 hours using a paint shaker manufactured by Toyo Seiki Co., Ltd. to obtain a cyan pigment dispersion (RMG1).
[0162] <Comparative Examples 1 to 3>
[0163] Cyan pigment dispersions (RMG2) to (RMG4) were obtained in the same manner as in Example 1 except that the zinc phthalocyanine halide pigments (RP2) to (RP4) were used instead of the zinc phthalocyanine halide pigment (RP1).
[0164] <Comparative Example 4>
[0165] A green pigment dispersion (SMG1) was obtained in the same manner as in Example 1 except that Pigment Green 7 (FASTOGEN Green S manufactured by DIC Corporation; hereinafter also referred to as “SP1”) was used instead of the zinc phthalocyanine halide pigment (RP1).
[0166] <Comparative Example 5>
[0167] According to [Production Example 3-6] of Japanese Patent Application Publication No. 2020-38368, β-zinc phthalocyanine (hereinafter also referred to as "SP2") was prepared. A cyan pigment dispersion (SMG2) was obtained in the same manner as in Example 1 except that (SP2) was used instead of the halogenated zinc phthalocyanine pigment (RP1).
[0168] <Evaluation of Color Filter Characteristics>
[0169] (Preparation of Evaluation Composition (RCG))
[0170] 0.98 g of UNIDIC ZL-295 (manufactured by DIC Corporation, trade name, solid content: 40% by mass) and 0.22 g of propylene glycol monomethyl ether acetate were added to 4.0 g of cyan pigment dispersion (RMG1), and mixed using a paint shaker to obtain an evaluation composition (RCG1) for evaluating the monochromatic chromaticity of a green pixel portion for a color filter. In addition, (RMG2) to (RMG4) and (SMG1) to (SMG2) were used instead of (RMG1), and the evaluation compositions (RCG2) to (RCG4) and (SCG1) to (SCG2) were prepared in the same manner as above.
[0171] (Preparation of Toning Composition (TY))
[0172] 1.65 g of CI Pigment Yellow 139 (Paliotol Yellow D1819 manufactured by BASF Corporation) was dispersed together with 3.85 g of DISPERBYK-161 (manufactured by BYK-Chemie, solid content: 30% by mass) and 11.00 g of propylene glycol monomethyl ether acetate using zirconium beads of 0.3 to 0.4 mm in a paint shaker for 2 hours to obtain a yellow pigment dispersion (MY1). 0.98 g of UNIDIC ZL-295 (manufactured by DIC Corporation, trade name, solid content: 40% by mass) and 0.22 g of propylene glycol monomethyl ether acetate were added to 4.0 g of the yellow pigment dispersion (MY1), and the mixture was mixed in a paint shaker to obtain a coloring composition (TY1).
[0173] <Light Source>
[0174] The light sources used in the embodiments and comparative examples are as follows. The spectra of light source A and light source B are as follows: Figure 2As described above, the color filter of the present invention can show chromaticity coordinates close to BT2020 in the XYZ color system of CIE, that is, 0.140≤chromaticity x≤0.200, 0.600≤chromaticity y≤0.797. In the embodiment of the present invention, (x, y)=(0.170, 0.750) in the color domain is set as the target chromaticity coordinates.
[0175] Light source A. LED+QD‥The light source described in Figure 5(a) of the paper "Langmuir 2017, 33, 13040-13050"
[0176] Light source B. LED KSF‥Model “NFSW157J-HG” manufactured by Nichia Chemical Corporation (For light source A: Preparation of evaluation composition (RDG) (SDG))
[0177] Evaluation compositions (RCG1) to (RCG4) and (SCG1) to (SCG2) were mixed with a coloring composition (TY1) to prepare evaluation compositions (RDG1) to (RDG4) and (SDG1) to (SDG2) for evaluating the performance of a green pixel portion for a color filter. Evaluation compositions (RDG1) to (RDG4) and (SDG1) to (SDG2) were spin-coated on a soda glass substrate and dried at 90° C. for 3 minutes to prepare an evaluation glass substrate having a colored film on the soda glass substrate. It should be noted that the mixing ratio of the evaluation composition (RCG1) to (RCG4) / the coloring composition (TY1), the mixing ratio of the evaluation composition (SCG1) to (SCG2) / the coloring composition (TY1) and the film thickness of the coating film were determined in such a way that the chromaticity of the coating film (measured using a spectrophotometer U-3900 manufactured by Hitachi High-Technologies Corporation) was (x, y) = (0.170, 0.750) when the light source A.LED+QD was used. The film thickness of the coating film was adjusted by adjusting the rotation speed during spin coating.
[0178] (evaluate)
[0179] The brightness Y of the coating film was measured using a spectrophotometer (U-3900) manufactured by Hitachi High-Technologies Corporation.
[0180] [Table 2]
[0181]
[0182] (For Light Source B: Preparation of Evaluation Composition (REG) (SEG))
[0183] Evaluation compositions (RCG1) to (RCG4) and (SCG1) to (SCG2) were mixed with a coloring composition (TY1) to prepare evaluation compositions (REG1) to (REG4) and (SEG1) to (SEG2) for evaluating the performance of a green pixel portion for a color filter. Evaluation compositions (REG1) to (REG4) and (SEG1) to (SEG2) were spin-coated on a soda glass substrate and dried at 90° C. for 3 minutes to prepare an evaluation glass substrate having a colored film on the soda glass substrate. It should be noted that the mixing ratio of the evaluation composition (RCG1) to (RCG4) / the coloring composition (TY1), the mixing ratio of the evaluation composition (SCG1) to (SCG2) / the coloring composition (TY1) and the film thickness of the coating film were determined so that the chromaticity of the coating film (measured using a spectrophotometer U-3900 manufactured by Hitachi High-Technologies Corporation) was (x, y) = (0.170, 0.750) when the light source B.LED KSF was used. The film thickness of the coating film was adjusted by adjusting the rotation speed during spin coating.
[0184] (evaluate)
[0185] The brightness Y of the coating film was measured using a spectrophotometer (U-3900) manufactured by Hitachi High-Technologies Corporation.
[0186] [Table 3]
[0187]
[0188] As shown in Tables 2 and 3, even when the light source was changed, Example 1 had higher brightness than Comparative Examples 1 to 5, confirming that the zinc phthalocyanine halide pigment (RP1) was superior to the zinc phthalocyanine halide pigments (RP2) to (RP4) and (SP1) to (SP2).
[0189] <Synthesis of Halogenated Zinc Phthalocyanine Pigments>
[0190] Halogenated zinc phthalocyanine pigments (RP5) to (RP8) were synthesized by the methods of the following Synthesis Examples 5 to 8. The average atomic number of halogen atoms in each pigment is shown in Table 4.
[0191] [Synthesis example 5]
[0192] 190 g of sulfonyl chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 315 g of aluminum chloride (manufactured by Kanto Chemical Co., Ltd.), 43 g of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), 84 g of zinc phthalocyanine (manufactured by DIC Corporation) and 116 g of bromine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 1L flask. The mixture was heated to 55°C, and after being taken out into water, it was filtered, washed with water and dried to obtain zinc phthalocyanine halide (R5). 40 g of zinc phthalocyanine halide (R5), 400 g of crushed sodium chloride and 63 g of 1,3-butanediol (melting point: -54°C) were added to a double-arm kneader, and the cooling water circulation device was set to -20°C, and kneaded for 20 hours. The kneaded mixture was taken out into 2 kg of water at 80°C and stirred for 1 hour. Then, the mixture was filtered, washed with hot water, dried, and crushed to obtain a halogenated zinc phthalocyanine pigment (RP5) as a cyan pigment. The halogenated zinc phthalocyanine pigment (RP5) was subjected to the same operation as in Synthesis Example 1 to calculate the average number of chlorine atoms and the average number of bromine atoms. In the halogenated zinc phthalocyanine pigment (RP5), the average number of halogen atoms in one molecule was 4.7, of which the average number of bromine atoms was 4.4 and the average number of chlorine atoms was 0.3.
[0193] [Synthesis example 6]
[0194] 270 g of sulfonyl chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 315 g of aluminum chloride (manufactured by Kanto Chemical Co., Ltd.), 86 g of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), 84 g of zinc phthalocyanine (manufactured by DIC Corporation) and 116 g of bromine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 1L flask. The mixture was heated to 70°C, taken out into water, filtered, washed with water and dried to obtain zinc phthalocyanine halide (R6). 40 g of zinc phthalocyanine halide (R6), 400 g of crushed sodium chloride and 63 g of 1,3-butanediol (melting point: -54°C) were added to a double-arm kneader, and the cooling water circulation device was set to -20°C, and kneaded for 20 hours. The kneaded mixture was taken out into 2 kg of water at 80°C and stirred for 1 hour. Then, the mixture was filtered, washed with hot water, dried, and crushed to obtain a halogenated zinc phthalocyanine pigment (RP6) as a cyan pigment. The halogenated zinc phthalocyanine pigment (RP6) was subjected to the same operation as in Synthesis Example 1 to calculate the average number of chlorine atoms and the average number of bromine atoms. In the halogenated zinc phthalocyanine pigment (RP6), the average number of halogen atoms in one molecule was 5.7, of which the average number of bromine atoms was 4.2 and the average number of chlorine atoms was 1.5.
[0195] [Synthesis Example 7]
[0196] 216 g of sulfonyl chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 315 g of aluminum chloride (manufactured by Kanto Chemical Co., Ltd.), 64 g of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), 84 g of zinc phthalocyanine (manufactured by DIC Corporation) and 162 g of bromine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 1L flask. The mixture was heated to 70°C, taken out into water, filtered, washed with water and dried to obtain zinc phthalocyanine halide (R7). 40 g of zinc phthalocyanine halide (R7), 400 g of crushed sodium chloride and 63 g of 1,3-butanediol (melting point: -54°C) were added to a double-arm kneader, and the cooling water circulation device was set to -20°C, and kneaded for 20 hours. The kneaded mixture was taken out into 2 kg of water at 80°C and stirred for 1 hour. Then, the mixture was filtered, washed with hot water, dried, and crushed to obtain a halogenated zinc phthalocyanine pigment (RP7) as a cyan pigment. The halogenated zinc phthalocyanine pigment (RP7) was subjected to the same operation as in Synthesis Example 1 to calculate the average number of chlorine atoms and the average number of bromine atoms. In the halogenated zinc phthalocyanine pigment (RP7), the average number of halogen atoms in one molecule was 6.8, of which the average number of bromine atoms was 6.1 and the average number of chlorine atoms was 0.7.
[0197] [Synthesis example 8]
[0198] 216 g of sulfonyl chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 315 g of aluminum chloride (manufactured by Kanto Chemical Co., Ltd.), 64 g of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd.), 84 g of zinc phthalocyanine (manufactured by DIC Corporation) and 209 g of bromine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 1L flask. The mixture was heated to 70°C, taken out into water, filtered, washed with water and dried to obtain zinc phthalocyanine halide (R8). 40 g of zinc phthalocyanine halide (R8), 400 g of crushed sodium chloride and 63 g of 1,3-butanediol (melting point: -54°C) were added to a double-arm kneader, and the cooling water circulation device was set to -20°C, and kneaded for 20 hours. The kneaded mixture was taken out into 2 kg of water at 80°C and stirred for 1 hour. Then, the mixture was filtered, washed with hot water, dried, and crushed to obtain a halogenated zinc phthalocyanine pigment (RP8) as a cyan pigment. The average number of chlorine atoms and the average number of bromine atoms were calculated for the halogenated zinc phthalocyanine pigment (RP8) in the same manner as in Synthesis Example 1. In the halogenated zinc phthalocyanine pigment (RP8), the average number of halogen atoms in one molecule was 8.9, of which the average number of bromine atoms was 8.4 and the average number of chlorine atoms was 0.5.
[0199] [Table 4]
[0200]
[0201] <Examples 2 to 6>
[0202] Cyan pigment dispersions (RMG5) to (RMG8) were obtained in the same manner as in Example 1 except that the zinc phthalocyanine halide pigments (RP5) to (RP8) were used instead of the zinc phthalocyanine halide pigment (RP1).
[0203] <Evaluation of Color Filter Characteristics>
[0204] (Preparation of Evaluation Composition (RCG))
[0205] 0.98 g of UNIDIC ZL-295 (manufactured by DIC Corporation, trade name, solid content: 40% by mass) and 0.22 g of propylene glycol monomethyl ether acetate were added to 4.0 g of cyan pigment dispersion (RMG5), and mixed using a paint shaker to obtain an evaluation composition (RCG5) for evaluating the performance of a green pixel portion for a color filter. In addition, (RMG6) to (RMG8) were used instead of (RMG5), and the evaluation compositions (RCG6) to (RCG8) were prepared in the same manner as above.
[0206] (Preparation of Toning Composition (TY))
[0207] CI Pigment Yellow 185 (Paliotol Yellow D1155 manufactured by BASF Corporation) 1.65 g, DISPERBYK-161 (manufactured by BYK-Chemie, solid content: 30% by mass) 3.85 g and propylene glycol monomethyl ether acetate 11.00 g were dispersed together with 0.3 to 0.4 mm zirconium beads in a paint shaker for 2 hours to obtain a yellow pigment dispersion (MY2). 0.98 g of UNIDIC ZL-295 (manufactured by DIC Corporation, trade name, solid content: 40% by mass) and 0.22 g of propylene glycol monomethyl ether acetate were added to 4.0 g of the yellow pigment dispersion (MY2), and mixed in a paint shaker to obtain a coloring composition (TY2). In addition, CI Pigment Yellow 138 (manufactured by BASF Corporation, Paliotol Yellow K0961HD) was used instead of CI Pigment Yellow 185, and the evaluation composition (TY3) was prepared in the same manner as above. In addition, the quinophthalone compound (D) described in the examples of International Publication 2018 / 159372 (Japanese Patent Application 2018-560690) was used instead of CI Pigment Yellow 185, and the evaluation composition (TY4) was prepared in the same manner as above.
[0208] (For Light Source A: Preparation of Evaluation Composition (RFG))
[0209] Evaluation compositions (RCG1) to (RCG2) and (RCG5) to (RCG8) were mixed with a coloring composition (TY2) to prepare evaluation compositions (RFG1) to (RFG2) and (RFG5) to (RFG8) for evaluating the performance of a green pixel portion for a color filter. Evaluation compositions (RFG1) to (RFG2) and (RFG5) to (RFG8) were spin-coated on a soda glass substrate and dried at 90° C. for 3 minutes to prepare an evaluation glass substrate having a colored film on the soda glass substrate. It should be noted that the mixing ratio of the evaluation composition (RFG1) to (RFG2) / the coloring composition (TY2), the mixing ratio of the evaluation composition (RFG5) to (RFG8) / the coloring composition (TY2) and the film thickness of the coating film were determined in such a way that the chromaticity of the coating film (measured using a spectrophotometer U-3900 manufactured by Hitachi High-Technologies Corporation) was (x, y) = (0.170, 0.750) when the light source A.LED+QD was used. The film thickness of the coating film was adjusted by adjusting the rotation speed during spin coating.
[0210] (evaluate)
[0211] The brightness Y of the coating film was measured using a spectrophotometer (U-3900) manufactured by Hitachi High-Technologies Corporation.
[0212] [Table 5]
[0213]
[0214] (For Light Source A: Preparation of Evaluation Composition (RGG))
[0215] Evaluation compositions (RCG1) to (RCG2) and (RCG5) to (RCG8) were mixed with a coloring composition (TY3) to prepare evaluation compositions (RGG1) to (RGG2) and (RGG5) to (RGG8) for evaluating the performance of a green pixel portion for a color filter. Evaluation compositions (RGG1) to (RGG2) and (RGG5) to (RGG8) were spin-coated on a soda glass substrate and dried at 90° C. for 3 minutes to prepare an evaluation glass substrate having a colored film on the soda glass substrate. It should be noted that the mixing ratio of the evaluation composition (RGG1) to (RGG2) / the coloring composition (TY3), the mixing ratio of the evaluation composition (RGG5) to (RGG8) / the coloring composition (TY3) and the film thickness of the coating film were determined in such a way that the chromaticity of the coating film (measured using a spectrophotometer U-3900 manufactured by Hitachi High-Technologies Corporation) was (x, y) = (0.170, 0.750) when the light source A.LED+QD was used. The film thickness of the coating film was adjusted by adjusting the rotation speed during spin coating.
[0216] (evaluate)
[0217] The brightness Y of the coating film was measured using a spectrophotometer (U-3900) manufactured by Hitachi High-Technologies Corporation.
[0218] [Table 6]
[0219]
[0220] (For Light Source A: Preparation of Evaluation Composition (RHG))
[0221] Evaluation compositions (RCG1) to (RCG2) and (RCG5) to (RCG8) were mixed with a coloring composition (TY4) to prepare evaluation compositions (RHG1) to (RHG2) and (RHG5) to (RHG8) for evaluating the performance of a green pixel portion for a color filter. Evaluation compositions (RHG1) to (RHG2) and (RHG5) to (RHG8) were spin-coated on a soda glass substrate and dried at 90° C. for 3 minutes to prepare an evaluation glass substrate having a colored film on the soda glass substrate. It should be noted that the mixing ratio of the evaluation composition (RHG1) to (RHG2) / the coloring composition (TY4), the mixing ratio of the evaluation composition (RHG5) to (RHG8) / the coloring composition (TY4) and the film thickness of the coating film were determined in such a way that the chromaticity of the coating film (measured using a spectrophotometer U-3900 manufactured by Hitachi High-Technologies Corporation) was (x, y) = (0.170, 0.750) when the light source A.LED+QD was used. The film thickness of the coating film was adjusted by adjusting the rotation speed during spin coating.
[0222] (evaluate)
[0223] The brightness Y of the coating film was measured using a spectrophotometer (U-3900) manufactured by Hitachi High-Technologies Corporation.
[0224] [Table 7]
[0225]
[0226] As shown in Tables 5 to 7, even when the yellow pigment used for coloring was changed, Examples 2 to 6 had higher brightness than Comparative Example 6, confirming that the zinc phthalocyanine halide pigments (RP1) and (RP5) to (RP8) were superior to the zinc phthalocyanine halide pigment (RP2).
[0227] <Reference Examples 1 to 8>
[0228] <Evaluation of color tone of color filter>
[0229] (Fabrication of Evaluation Substrate)
[0230] The evaluation compositions (RCG1) to (RCG8) and (SCG2) were spin-coated on a soda glass substrate, dried at 90°C for 3 minutes, and then heated at 230°C for 1 hour. Thus, an evaluation glass substrate having a colored film on a soda glass substrate was prepared. It should be noted that the film thickness of the colored film obtained by heating at 230°C for 1 hour was adjusted by adjusting the rotation speed during spin coating. For each reference example, an evaluation glass substrate with a colored film thickness of 1.5 μm, an evaluation glass substrate with a colored film thickness of 1.9 μm, and an evaluation glass substrate with a colored film thickness of 2.4 μm were prepared. The film thickness was measured using a white interference microscope (VS1330) manufactured by Hitachi High-Technologies Corporation.
[0231] (evaluate)
[0232] For each glass substrate for evaluation, the chromaticity (x, y) of the colored film under light source C was measured using a spectrophotometer (U-3900) manufactured by Hitachi High-Technologies Corporation. The results are shown in Table 8. Figure 3 As shown in FIG. 1 , the chromaticity (x, y) of the obtained colored film is plotted on the xy chromaticity coordinates in the XYZ color system of CIE. Figure 3 The chromaticity coordinate region A enclosed by the following formulas (A) to (D), the xy chromaticity coordinate region B enclosed by the following formulas (C) and (E) to (G), and the xy chromaticity coordinate region C enclosed by the following formulas (E) and (H) to (J) are shown. Figure 3 The three marks of RCG1, 5 to 8, RCG2 to 4, and SCG2 respectively represent the coordinates when the film thickness is 1.5, 1.9, and 2.4 μm.
[0233] Formula (A): y = -1.766x + 0.618
[0234] (where x is 0.10≤x≤0.17)
[0235] Formula (B): y = 5.889x - 0.683
[0236] (where x is 0.15≤x≤0.17)
[0237] Formula (C): y = 0.125x + 0.181
[0238] (where x is 0.07≤x≤0.15)
[0239] Formula (D): y = 8.380x - 0.397
[0240] (where x is 0.07≤x≤0.10)
[0241] Formula (E): y = -1.333x + 0.503
[0242] (where x is 0.10≤x≤0.16)
[0243] Formula (F): y = 9.000x - 1.150
[0244] (where x is 0.15≤x≤0.16)
[0245] Formula (G): y = 6.000x - 0.230
[0246] (where x is 0.07≤x≤0.10)
[0247] Formula (H): y = 7.000x - 0.830
[0248] (where x is 0.15≤x≤0.16)
[0249] Formula (I): y = -0.286x + 0.263
[0250] (where x is 0.08≤x≤0.15)
[0251] Formula (J): y = 6.500x - 0.280
[0252] (Wherein, x is 0.08≤x≤0.10).
[0253] [Table 8]
[0254]
[0255] In the above Table 8, (RP1), (RP5) to (RP8) used in Reference Examples 1, 5 to 8 are pigments of the present invention (Examples). On the other hand, RP4 and SP2 used in Reference Examples 4 and 9 are pigments outside the scope of the present invention (Comparative Examples). Figure 3 It can be seen that (RCG1), (RCG5) to (RCG8) can show the xy chromaticity coordinate area surrounded by formulas (A) to (D) in the XYZ colorimetric system of CIE when the color is measured using the C light source alone when the film thickness is 1.5 μm to 2.4 μm and the composition is set to 1.25 parts of resin per part of pigment in terms of mass conversion. Based on the above results, it can be confirmed that the number of halogen atoms in one molecule is 0.2 to 10 on average, the number of bromine atoms is 0.1 to 10 on average, and the number of chlorine atoms is 0.1 to less than 2 on average. Furthermore, the halogenated zinc phthalocyanine pigments whose hue falls within the range surrounded by formulas (A) to (D) have higher brightness.
Claims
1. A color filter pigment, which is a pigment used to form a coating film in a green pixel portion of a color filter, When the film thickness of the coating film is set to 1.5 μm to 2.4 μm and the composition is set to 1.25 parts of resin per 1 part of the pigment in terms of mass conversion, in the XYZ colorimetric system of CIE when colorimetry is performed using only C light source, an xy chromaticity coordinate region surrounded by the following formulas (A) to (D) can be displayed: Formula (A) y=-1.766x+0.618 Wherein, x is 0.10≤x≤0.17; Formula (B) y=5.889x-0.683 Wherein, x is 0.15≤x≤0.17; Formula (C) y=0.125x+0.181 Wherein, x is 0.07≤x≤0.15; Formula (D) y=8.380x-0.397 Wherein, x is 0.07≤x≤0.10; The pigment comprises a compound represented by the following formula (1), namely, a halogenated zinc phthalocyanine pigment, wherein the number of halogen atoms in one molecule of the compound is 0.2 or more and 10 or less on average, the number of bromine atoms in one molecule of the compound is 0.1 or more and 10 or less on average, and the number of chlorine atoms in one molecule of the compound is 0.1 or more and less than 2 on average, In formula (1), X 1 ~X 16 Each independently represents a hydrogen atom or a halogen atom. 2 . The pigment for color filter according to claim 1 , wherein the number of bromine atoms in one molecule of the compound is 2.0 or more and 7.9 or less on average. 3 . The pigment for color filter according to claim 1 , wherein the number of halogen atoms in one molecule of the compound is 3.5 or more and 9.0 or less on average. 4 . The pigment for color filter according to claim 1 , wherein the number of chlorine atoms in one molecule of the compound is 0.2 or more and 1.6 or less on average. 5 . A coloring composition comprising the pigment for color filter according to claim 1 or 2 and a solvent. 6 . A color filter comprising a coating film formed of the color filter pigment according to claim 1 or 2 in a green pixel portion.