An oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst and its preparation method and application
The thioate salt is formed by reacting molybdenum or tungsten source with a sulfide source, and a sulfur-containing nickel molybdenum or nickel tungsten bimetallic salt composite is formed with a nickel source, and an oil-soluble bimetallic catalyst is prepared in combination with organic acids, which solves the problem of the existing technology. The problems of high temperature and vulcanizing agent addition have achieved high activity and low cost catalytic effects.
Patent Information
- Application Number
- CN202111598504.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-12-24
AI Technical Summary
The existing oil-soluble catalysts require high temperature and additional vulcanizing agents during the preparation process, resulting in reduced catalytic activity and increased operating costs. The preparation method of bimetallic catalysts is complex and uneven.
Molybdenum or tungsten source reacts with a vulcanizing agent to form a thioate salt, and then mixes it with a nickel source to form a sulfur-containing nickel molybdenum or nickel tungsten bimetallic salt composite, and reacts with an organic acid to produce oil-soluble nickel molybdenum or nickel tungsten bis The metal catalyst precursor forms a synergistic bimetallic catalyst through chemical bonding, reducing metal loss and uneven vulcanization.
Highly active and low-cost oil-soluble nickel-molybdenum or nickel-tungsten bimetallic catalysts are realized, which simplifies the preparation process, reduces metal loss and uneven vulcanization problems, improves hydrogenation activity and inhibits coking performance.
Smart Images

Figure BDA0003431045210000111 
Figure BDA0003431045210000121 
Figure BDA0003431045210000122
Abstract
Description
Technical Field
[0001] The invention relates to an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst and a preparation method and application thereof, belonging to the technical field of petrochemical industry. Background Art
[0002] Oil-soluble catalysts are catalysts with organic metal compounds that can dissolve in heavy oil as the active components of the catalyst. When the oil-soluble catalyst is added to the raw material, it first dissolves in the raw material and then decomposes into molecular-sized catalyst particles at a suitable temperature. Since the organic metal compound can be evenly dispersed in the heavy oil and fully contacted with the heavy oil and hydrogen, it can effectively inhibit the formation of coke. Under the same metal content, the catalytic effect of the oil-soluble catalyst is better than that of the water-soluble catalyst, and no emulsifier is required, making it an ideal catalyst.
[0003] At present, a variety of oil-soluble catalysts have been reported in the prior art. For example, Chinese patent CN106391111A discloses an oil-soluble catalyst and a preparation method thereof. The preparation method comprises: mixing a soluble salt of VIB group metals Mo and / or W, a soluble salt of at least one of VIII group metals Fe, Co or Ni, and water to obtain a mixed solution; adjusting the pH of the mixed solution to alkaline, and then performing a precipitation reaction at 40-100° C. to obtain an active metal precursor; and reacting the active metal precursor with an organic precursor compound in an oxygen-free atmosphere to obtain an oil-soluble catalyst.
[0004] The defects of this technology or the shortcomings relative to the present invention are: although this type of oil-soluble catalyst exhibits excellent hydrocracking performance, a sulfiding agent must be added to the precursor to be converted into a catalytically active metal sulfide. Due to the difficulty of sulfidation, the final sulfide particle size is large, which reduces the catalytic hydrogenation activity, leads to a large addition amount, and increases the cost of operation.
[0005] Chinese patent CN104888796A discloses an oil-soluble Mo-Ni bimetallic catalyst suitable for suspended bed hydrocracking of inferior residue oil, a preparation method and its use. The preparation method comprises: dissolving nickel nitrate and ammonium molybdate in distilled water, adding a small amount of ethylene glycol, adjusting the pH value to alkaline, heating the solution, reacting at 130-160°C to obtain a solid intermediate product, drying the solid intermediate product at 100°C under normal pressure, mixing with oleic acid, and reacting at 230-260°C to obtain an oil-soluble Mo-Ni bimetallic catalyst.
[0006] The defects of this technology or the shortcomings relative to the present invention are: the catalyst preparation process requires a high reaction temperature, which needs to be carried out at a temperature greater than 130°C and 230°C, and when the catalyst is used in a suspended bed hydrocracking reaction of super heavy oil atmospheric residue, an additional sulfiding agent needs to be added.
[0007] Chinese patent CN107469837A / CN107649152A discloses the use of molybdenum / tungsten thiomolybdates and organic acids to react in one step to prepare an oil-soluble molybdenum / tungsten-based catalyst precursor, the use of nickel salts and organic amines to react in one step to prepare an oil-soluble nickel-based catalyst precursor, and then adding a dispersant to achieve mutual solubility and stable dispersion of the nickel-based and molybdenum / tungsten-based catalyst precursors in inferior heavy oil, and self-sulfurization decomposition to form nano-scale dispersed active metal molybdenum sulfide modified with the auxiliary nickel.
[0008] The defects of this technology or the shortcomings relative to the present invention are: the method of adding two metal precursors separately and physically mixing two monometallic catalyst precursors to prepare a bimetallic catalyst.
[0009] Chinese patent CN108745385A discloses a method for preparing a self-sulfurized oil-soluble molybdenum-based bimetallic catalyst, comprising the following steps: a molybdenum source compound and a second metal salt are chemically precipitated to form a molybdenum-based bimetallic complex; the molybdenum-based bimetallic complex is treated with a sulfiding agent to obtain a bimetallic thiomolybdate; an oil-soluble molybdenum-based bimetallic catalyst precursor is prepared by reacting an organic amine with the bimetallic thiomolybdate; and a dispersant is added to the oil-soluble molybdenum-based bimetallic catalyst precursor to form a self-sulfurized oil-soluble molybdenum-based bimetallic catalyst.
[0010] The defects of this technology or the shortcomings relative to the present invention are as follows: the intermediate product, the molybdenum-based bimetallic complex, produced during the preparation process is a solid precipitate, which will cause metal loss during the washing, filtering and drying process and increase the reaction time; and in the subsequent treatment, a vulcanizing agent is required to vulcanize this solid intermediate product, and the vulcanization process is more complicated and may cause uneven vulcanization.
[0011] Therefore, providing a new type of oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst and its preparation method and application has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0012] In order to solve the above-mentioned shortcomings and deficiencies, an object of the present invention is to provide a method for preparing an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst.
[0013] Another object of the present invention is to provide an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst, which is prepared by the preparation method of the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst described above.
[0014] Another object of the present invention is to provide an application of the above-mentioned oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst in a slurry bed hydrocracking process of inferior heavy oil.
[0015] Another object of the present invention is to provide a slurry bed hydrocracking process for inferior heavy oil, which utilizes the above-mentioned oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst to carry out slurry bed hydrocracking of inferior heavy oil.
[0016] In order to achieve the above objectives, on the one hand, the present invention provides a method for preparing an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst, wherein the preparation method comprises:
[0017] S1: mixing a molybdenum source or a tungsten source with a sulfurizing agent and reacting the mixture to obtain thiomolybdate or thiotungstate;
[0018] S2: mixing thiomolybdate or thiotungstate with a nickel source and reacting the mixture to obtain a sulfur-containing nickel-molybdenum bimetallic salt complex or a sulfur-containing nickel-tungsten bimetallic salt complex;
[0019] S3: reacting a sulfur-containing nickel-molybdenum bimetallic salt complex or a sulfur-containing nickel-tungsten bimetallic salt complex with an organic acid to obtain a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst or a precursor of a nickel-tungsten bimetallic catalyst;
[0020] S4: dissolving a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst or a precursor of a nickel-tungsten bimetallic catalyst in an organic dispersant to obtain a precursor solution of a nickel-molybdenum bimetallic catalyst or a precursor solution of a nickel-tungsten bimetallic catalyst;
[0021] S5: dissolving a precursor solution of a nickel-molybdenum bimetallic catalyst or a precursor solution of a nickel-tungsten bimetallic catalyst in a dispersing oil to obtain an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst.
[0022] In the preparation method provided by the present invention, a sulfur-containing nickel-molybdenum bimetallic salt complex or a sulfur-containing nickel-tungsten bimetallic salt complex is reacted with an organic acid to obtain a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst or a precursor of a nickel-tungsten bimetallic catalyst. The bimetal in the precursor is chemically bonded, that is, it is a single catalyst composed of bimetals, and the synergistic effect between the bimetals is stronger, so that the catalyst can exhibit better hydrogenation activity and coke inhibition performance.
[0023] As a specific embodiment of the preparation method described above in the present invention, S1 includes: dissolving a molybdenum source or a tungsten source in ammonia water or water, and then adding a sulfiding agent to the resulting solution for reaction to obtain thiomolybdate or thiotungstate.
[0024] As a specific implementation of the above preparation method of the present invention, the ratio of the volume of the ammonia water to the mass of the molybdenum source or the tungsten source is 1-2:1, and the units are mL and g respectively.
[0025] As a specific embodiment of the preparation method described above in the present invention, the molybdenum source includes one or a combination of molybdenum trioxide, ammonium molybdate, ammonium heptamolybdate tetrahydrate, ammonium metamolybdate, and ammonium paramolybdate.
[0026] As a specific embodiment of the preparation method described above in the present invention, the tungsten source includes one or a combination of tungsten trioxide, ammonium tungstate, ammonium metatungstate, and ammonium paratungstate.
[0027] As a specific embodiment of the above preparation method of the present invention, the molar ratio of the sulfur content of the vulcanizing agent to molybdenum or tungsten is 2-6:1.
[0028] As a specific embodiment of the preparation method described above in the present invention, the sulfiding agent includes one or a combination of ammonium sulfide, sodium sulfide, and potassium sulfide.
[0029] In the preparation method provided by the present invention, depending on the different vulcanizing agents used, the thiomolybdate may be one or a combination of ammonium thiomolybdate, sodium thiomolybdate and potassium thiomolybdate; the thiotungstate may be one or a combination of ammonium thiotungstate, sodium thiotungstate and potassium thiotungstate.
[0030] As a specific embodiment of the preparation method described above of the present invention, the reaction temperature in S1 is 30-150° C., and the reaction time is 0.5-3 h.
[0031] As a specific embodiment of the preparation method described above in the present invention, S2 includes: dissolving the nickel source in excess ammonia water, and then mixing the obtained nickel source ammonia solution with the sulfur-containing molybdenum source or sulfur-containing tungsten source solution obtained in S1, and then reacting to obtain a sulfur-containing nickel-molybdenum bimetallic salt complex or a sulfur-containing nickel-tungsten bimetallic salt complex.
[0032] As a specific embodiment of the preparation method described above, the molar ratio of the ammonia water to the nickel source is 1-10: 1. The molar ratio of the ammonia water is calculated based on ammonia monohydrate.
[0033] As a specific embodiment of the preparation method described above in the present invention, the nickel source includes one or more nickel salts such as nickel nitrate, nickel acetate, basic nickel carbonate, nickel sulfate, and nickel formate.
[0034] As a specific embodiment of the preparation method described above of the present invention, in S2, the reaction temperature is 30-150° C., and the reaction time is 0.5-3 h.
[0035] As a specific embodiment of the preparation method described above in the present invention, wherein, between S2 and S3, it also includes: filtering and washing the product obtained from the reaction in S2, and drying at room temperature to obtain a precipitate, i.e., a sulfur-containing nickel-molybdenum bimetallic salt or a sulfur-containing nickel-tungsten bimetallic salt complex.
[0036] As a specific embodiment of the above preparation method of the present invention, the molar ratio of the organic acid to molybdenum or tungsten is 2-6:1.
[0037] As a specific embodiment of the above preparation method of the present invention, the organic acid includes one or more of alkane acid, cycloalkane acid, oleic acid and linoleic acid.
[0038] As a specific embodiment of the preparation method described above of the present invention, in S3, the reaction temperature is 50-200° C., and the reaction time is 0.5-5 h.
[0039] As a specific embodiment of the above preparation method of the present invention, the molar ratio of the organic dispersant to molybdenum or tungsten is 0.1-1:1.
[0040] As a specific embodiment of the preparation method described above of the present invention, the organic dispersant comprises one or more of tetralin, decalin, tetrahydrofuran, dimethyl sulfoxide, and aniline.
[0041] As a specific embodiment of the preparation method described above in the present invention, the mass ratio of the dispersing oil to the precursor solution of the nickel-molybdenum bimetallic catalyst or the precursor solution of the nickel-tungsten bimetallic catalyst is 1-10:1.
[0042] As a specific embodiment of the preparation method described above of the present invention, the dispersant oil includes one or a combination of straight-run gasoline, straight-run diesel, straight-run wax oil, catalytic cracking gasoline, catalytic cracking diesel, catalytic cracking wax oil, catalytic cracking slurry, coker gasoline, coker diesel, coker wax oil, hydrocracking gasoline, hydrocracking diesel, and hydrocracking wax oil.
[0043] On the other hand, the present invention also provides an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst, wherein the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst is prepared by the preparation method of the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst described above;
[0044] Wherein, based on the total weight of the catalyst being 100%, the mass percentage of tungsten or molybdenum is 1-20%, and the mass percentage of nickel is 1-12%.
[0045] The oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst provided by the present invention is a highly active new self-sulfurized oil-soluble inferior heavy oil slurry bed hydrocracking catalyst with the characteristics of simple preparation process, no need for sulfurization, and small amount of catalyst added during application.
[0046] On the other hand, the present invention also provides the use of the above-mentioned oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst in a low-quality heavy oil slurry bed hydrocracking process.
[0047] On the other hand, the present invention also provides a slurry bed hydrocracking process for inferior heavy oil, wherein the process utilizes the above-mentioned oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst to carry out slurry bed hydrocracking of inferior heavy oil.
[0048] As a specific embodiment of the process described above of the present invention, for each gram of inferior heavy oil, the amount of the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst is 200-2000 μg in terms of metal molybdenum or tungsten, and 50-1000 μg in terms of metal nickel;
[0049] The operating conditions of the slurry bed hydrogenation reactor used in the process are: reaction pressure 5-25MPa, reaction temperature 380-450°C, volume space velocity 0.2-1.2h -1 , hydrogen-oil volume ratio 200-1500.
[0050] Among them, the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst provided by the present invention is particularly suitable for the slurry bed hydrocracking process of inferior heavy oil with high metal content, high carbon content and high sulfur content, with a metal (Ni, V, Fe and Ca) content of not less than 200 ppm or a carbon residue of not less than 10wt% or a sulfur content of not less than 3wt%.
[0051] During the application process, the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst provided by the present invention is added to low-quality heavy oil. The precursor of the catalyst is dispersed in the low-quality heavy oil and can self-sulfurize and decompose to form active metal molybdenum sulfide or tungsten sulfide modified with active metal nickel and dispersed at the nanoscale.
[0052] Compared with the prior art, the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst provided by the present invention can achieve the following technical effects:
[0053] The present invention adopts a sulfur-containing nickel-molybdenum bimetallic salt complex or a sulfur-containing nickel-tungsten bimetallic salt complex to react with an organic acid to obtain a sulfur-substituted oil-soluble nickel-molybdenum bimetallic catalyst precursor or a nickel-tungsten bimetallic catalyst precursor. Compared with the bimetallic catalyst prepared by physically mixing two monometallic catalyst precursors in the prior art, a chemical bond is formed between the two oxygen atoms of the carboxylate in the organic ligand and the nickel atom to form a structure with a layered structure and an internal void space, which is conducive to the exposure of more active sites. The synergistic effect between the bimetals in the bimetallic catalyst with this specific structure provided by the present invention is stronger, thereby showing better hydrogenation activity and coke inhibition performance.
[0054] The present invention first uses a molybdenum source or a tungsten source and a vulcanizing agent to react chemically in an ammonia system or a water system to generate a liquid intermediate product, that is, a solution containing thiomolybdate or thiotungstate, and then adds a nickel source to react to generate a precipitate. The entire process only undergoes one precipitation step, which greatly reduces the metal loss caused by the treatment of solid intermediate products in the production process, and also reduces the generation of washing wastewater, and the vulcanization is more uniform.
[0055] In addition, the present invention also uses an organic dispersant and a dispersant oil when preparing the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst, which can achieve rapid and stable dispersion of the catalyst precursor in inferior heavy oil. No additional vulcanizing agent is required, and active metal molybdenum / tungsten sulfide modified with nano-nickel sulfide can be generated by in-situ decomposition. The synthesis process is simple, the conditions are mild, and it is convenient for large-scale industrial production. DETAILED DESCRIPTION
[0056] It should be noted that the term "comprises" and any variations thereof in the specification and claims of the present invention are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or devices.
[0057] "Scope" disclosed in the present invention is given in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges defined in this way are combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, for a specific parameter, a range of 60-120 and 80-110 is listed, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values listed are 1 and 2, and the maximum range values listed are 3, 4 and 5, then the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.
[0058] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in the present invention, and "0-5" is just an abbreviation of these numerical combinations.
[0059] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned in the present invention can be combined with each other to form a new technical solution.
[0060] In the present invention, unless otherwise specified, all technical features and preferred features mentioned in the present invention can be combined with each other to form a new technical solution.
[0061] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the attached table and examples. The following described embodiments are some embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0062] Example 1
[0063] This embodiment provides an oil-soluble nickel-tungsten bimetallic catalyst, which is prepared according to a preparation method comprising the following steps:
[0064] S1: Weigh 30g of tungsten trioxide, add 200mL of distilled water, then add 60mL of concentrated ammonia water, stir, and heat to 40°C to dissolve. Add ammonium sulfide solution with a sulfur content of 8wt% to the solution under stirring (wherein, the molar ratio of the sulfur content of the sulfiding agent to tungsten in this embodiment is 4:1), heat to 80°C, stir and react for 2 hours to obtain solution A containing ammonium thiotungstate.
[0065] S2: Weigh 37.5 g of nickel nitrate hexahydrate, add ammonia water, and the molar ratio of ammonia water to nickel is 10 / 1 to obtain solution B. Under stirring conditions, solution B is added to solution A and reacted, wherein the reaction temperature is 90° C. and the reaction time is 2 hours to generate precipitate C. The precipitate is filtered, washed with water, and dried at room temperature to obtain nickel ammonium thiotungstate, a total of 59.88 g, with a yield of 98.2%.
[0066] S3: Weigh 5 g of ammonium nickel thiotungstate and add it to oleic acid for reaction, wherein the molar ratio of oleic acid to tungsten is 4 / 1, the reaction temperature is 90°C, and the reaction time is 1 hour. After the reaction, the precursor of the oil-soluble nickel-tungsten bimetallic catalyst is obtained, which is named NW-1.
[0067] S4: dissolving the precursor of the oil-soluble nickel-tungsten bimetallic catalyst in the organic dispersant tetrahydrofuran, wherein the molar ratio of tetrahydrofuran / tungsten is 0.5 / 1, to obtain the precursor solution S-1 of the oil-soluble nickel-tungsten bimetallic catalyst.
[0068] S5: The solution S-1 was dissolved in hydrocracked diesel, with the ratio of hydrocracked diesel / S-1 solution = 4 / 1 (g / g), to obtain an oil-soluble nickel-tungsten bimetallic catalyst solution, named Y-NW-1.
[0069] Example 2
[0070] This embodiment provides an oil-soluble nickel-tungsten bimetallic catalyst, which is prepared according to a preparation method comprising the following steps:
[0071] S1: Weigh 30g of ammonium metatungstate and 150g of sodium sulfide nonahydrate, add 250mL of distilled water, stir, heat to 60°C to dissolve, heat to 70°C, stir and react for 2 hours to obtain solution A containing sodium thiotungstate.
[0072] S2: Weigh 18g of nickel formate, add ammonia water, the molar ratio of ammonia water / nickel = 10 / 1, and obtain solution B. Under stirring conditions, add solution B to solution A and react, wherein the reaction temperature is 90°C and the reaction time is 2 hours to generate precipitate C. The precipitate is filtered, washed with water, and dried at room temperature to obtain nickel ammonium thiotungstate, a total of 56.06g, with a yield of 98%.
[0073] S3: Weigh 5 g of ammonium nickel thiotungstate and add it to linoleic acid for reaction. The molar ratio of linoleic acid to tungsten is 4 / 1. The reaction temperature is 140°C and the reaction time is 2.5 hours. After the reaction, the precursor of the oil-soluble nickel-tungsten bimetallic catalyst is obtained, which is named NW-2.
[0074] S4: dissolving the precursor of the oil-soluble nickel-tungsten bimetallic catalyst in the organic dispersant decahydronaphthalene, with the molar ratio of decahydronaphthalene to tungsten being 1 / 1, to obtain a precursor solution S-2 of the oil-soluble nickel-tungsten bimetallic catalyst.
[0075] S5: The solution S-2 was dissolved in coker gasoline, coker gasoline / S-2 solution = 4 / 1 (g / g), to obtain an oil-soluble nickel-tungsten bimetallic catalyst solution, named Y-NW-2.
[0076] Example 3
[0077] This embodiment provides an oil-soluble nickel-molybdenum bimetallic catalyst, which is prepared according to a preparation method comprising the following steps:
[0078] S1: Weigh 30g of molybdenum trioxide, add 200mL of distilled water, then add 60mL of concentrated ammonia water, stir, and heat to 40°C to dissolve. Add an ammonium sulfide solution with a sulfur content of 8wt% to the solution under stirring (wherein, the molar ratio of the sulfur content of the sulfiding agent to molybdenum in this embodiment is 2:1), heat to 80°C, stir and react for 2 hours to obtain a solution A containing ammonium thiomolybdate.
[0079] S2: Weigh 60g of nickel nitrate hexahydrate, add ammonia water, ammonia water / nickel molar ratio = 10 / 1, and obtain solution B. Under stirring conditions, solution B is added to solution A for reaction, wherein the reaction temperature is 90°C and the reaction time is 2 hours to generate precipitate C. The precipitate is filtered, washed with water, and dried at room temperature for 12 hours to obtain nickel ammonium thiomolybdate, a total of 78.72g, with a yield of 98.4%.
[0080] S3: Weigh 5 g of nickel ammonium thiomolybdate and add it to oleic acid for reaction, wherein the molar ratio of oleic acid / molybdenum is 4 / 1, the reaction temperature is 90° C., and the reaction time is 1 hour, to obtain a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst, named NM-1.
[0081] S4: The precursor of the oil-soluble nickel-molybdenum bimetallic catalyst is dissolved in the organic dispersant tetrahydrofuran, and the molar ratio of tetrahydrofuran to molybdenum is 0.5 / 1 to obtain the precursor solution S-3 of the oil-soluble nickel-molybdenum bimetallic catalyst.
[0082] S5: The solution S-3 was dissolved in catalytic cracking diesel, catalytic cracking diesel / S-3 solution = 4 / 1 (g / g), to obtain an oil-soluble nickel-molybdenum bimetallic catalyst solution, named Y-NM-1.
[0083] Example 4
[0084] This embodiment provides an oil-soluble nickel-molybdenum bimetallic catalyst, which is prepared according to a preparation method comprising the following steps:
[0085] S1: Weigh 27 g of ammonium heptamolybdate tetrahydrate, add 150 mL of distilled water, then add 50 mL of concentrated aqueous ammonia, stir, and heat to 60° C. to dissolve. Add an ammonium sulfide solution with a sulfur content of 8 wt% to the solution under stirring (wherein, the molar ratio of the sulfur content of the sulfiding agent to molybdenum in this embodiment is 6:1), heat to 85° C., stir and react for 1.5 hours to obtain a solution A containing ammonium thiomolybdate.
[0086] S2: Weigh 40g of nickel acetate tetrahydrate, add ammonia water, ammonia water / nickel molar ratio = 8 / 1, to obtain solution B. Under stirring conditions, solution B is added to solution A for reaction, wherein the reaction temperature is 90°C and the reaction time is 2 hours to generate precipitate C. The precipitate is filtered, washed with water, and dried at room temperature to obtain nickel ammonium thiomolybdate, a total of 57.68g, with a yield of 98%.
[0087] S3: Weigh 5 g of nickel ammonium thiomolybdate and add it to cyclohexane acid for reaction, wherein the molar ratio of cyclohexane acid to molybdenum is 4 / 1, the reaction temperature is 120°C, and the reaction time is 2 hours. After the reaction, a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst is obtained, which is named NM-2.
[0088] S4: Dissolve the precursor of the oil-soluble nickel-molybdenum bimetallic catalyst in the organic dispersant aniline, wherein the molar ratio of aniline / molybdenum is 1 / 1, to obtain the precursor solution S-4 of the oil-soluble nickel-molybdenum bimetallic catalyst.
[0089] S5: Dissolve the solution S-4 in hydrocracking wax oil, wherein the hydrocracking wax oil / S-4 solution = 4 / 1 (g / g), to obtain an oil-soluble nickel-molybdenum bimetallic catalyst solution, named Y-NM-2.
[0090] Reference Example 1
[0091] This reference example provides an oil-soluble tungsten-based catalyst, which is prepared according to a preparation method comprising the following steps:
[0092] Weigh 5 g of ammonium thiotungstate and add it to dodecanoic acid for reaction, wherein the molar ratio of dodecanoic acid to tungsten is 2.5 / 1, the reaction temperature is 90° C., and the reaction time is 1 hour, thereby obtaining a precursor of an oil-soluble tungsten-based catalyst, named W-1.
[0093] The precursor of the oil-soluble tungsten-based catalyst was dissolved in the organic dispersant tetrahydrofuran, wherein the molar ratio of tetrahydrofuran to tungsten was 0.5 / 1, to obtain a solution S-5.
[0094] The solution S-5 was dissolved in catalytic cracking diesel, wherein the catalytic cracking diesel / S-5 solution = 4 / 1 (g / g), to obtain an oil-soluble tungsten-based catalyst solution, named CW-1.
[0095] Reference Example 2
[0096] This reference example provides an oil-soluble nickel-molybdenum bimetallic catalyst, which is prepared according to a preparation method comprising the following steps:
[0097] Weigh 30g of molybdenum trioxide, add 200mL of distilled water, and then add 60mL of concentrated ammonia water to obtain solution A. Weigh 60g of nickel nitrate hexahydrate, add ammonia water, ammonia water / nickel molar ratio = 10 / 1, and obtain solution B. Under stirring conditions, solution B is added to solution A for reaction, wherein the reaction temperature is 60°C, the reaction time is 4 hours, and a green precipitate is generated. The precipitate is filtered, washed with water, and dried at room temperature to obtain nickel ammonium molybdate. Then nickel ammonium molybdate is added to an ammonium sulfide solution with a sulfur content of 8% (wherein the molar ratio of the sulfur content of the vulcanizing agent to molybdenum in this reference ratio is 2:1), the temperature is raised to 80°C, and the reaction is stirred for 4 hours. The liquid containing the precipitate obtained after the reaction is filtered with a Buchner funnel, washed with distilled water, and left to dry at room temperature for 12 hours to obtain nickel ammonium thiomolybdate, a total of 77.44g, with a yield of 96.8%.
[0098] 5 g of nickel ammonium thiomolybdate was weighed and added to oleic acid for reaction, wherein the oleic acid / molybdenum molar ratio was 4 / 1, the reaction temperature was 90° C., and the reaction time was 1 hour. After the reaction, a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst was obtained, named NM-3.
[0099] The precursor of the oil-soluble nickel-molybdenum bimetallic catalyst was dissolved in the organic dispersant tetrahydrofuran, wherein the molar ratio of tetrahydrofuran to molybdenum was 0.5 / 1, to obtain the precursor solution S-6 of the oil-soluble nickel-molybdenum bimetallic catalyst.
[0100] The solution S-6 was dissolved in catalytic cracking diesel, wherein the catalytic cracking diesel / S-6 solution = 4 / 1 (g / g), to obtain an oil-soluble nickel-molybdenum bimetallic catalyst solution, named C-NM-3.
[0101] Reference Example 3
[0102] This reference example provides a dispersion containing molybdenum-based and nickel-based precursors, which is prepared according to a preparation method comprising the following steps:
[0103] Weigh 5 g of ammonium thiomolybdate and add it to oleic acid for reaction, wherein the oleic acid / molybdenum molar ratio is 4 / 1, the reaction temperature is 90° C., and the reaction time is 1 hour. After the reaction, a precursor of an oil-soluble molybdenum-based catalyst is obtained, named M-1.
[0104] Weigh 5g of nickel nitrate, add 20mL of distilled water, and stir to dissolve. Add dodecaamine to the solution under stirring to react, wherein the molar ratio of dodecaamine to nickel is 2.5 / 1, the reaction temperature is 50°C, and the reaction time is 1 hour. The liquid containing the precipitate obtained after the reaction is filtered with a Buchner funnel, washed with distilled water, and left to dry at room temperature for 12 hours to obtain a precursor of an oil-soluble nickel-based catalyst, named N-1.
[0105] Under stirring conditions, the oil-soluble molybdenum-based catalyst precursor M-1 is added to the dispersant catalytic cracking diesel, wherein the catalytic cracking diesel / M-1=3 / 1 (g / g). After complete dissolution, a certain amount of oil-soluble nickel-based catalyst precursor N-1 is added, and the nickel / molybdenum molar ratio is made to be 1 / 1, to obtain a dispersion containing molybdenum-based and nickel-based precursors, named C-MN-4.
[0106] Test Example 1
[0107] This test example evaluates the hydrocracking of vacuum residue oil using seven different oil-soluble catalyst solutions provided in Examples 1 to 4 and Reference Examples 1 to 3, specifically including:
[0108] Seven oil-soluble catalyst solutions (Y-NW-1, Y-NW-2, Y-NM-1, Y-NM-2, CW-1, C-NM-3, C-MN-4) in Example 1, Example 2, Example 3, Example 4, Reference Example 1, Reference Example 2 and Reference Example 3 were used as catalysts, respectively, and Middle East high sulfur vacuum residue oil was used as a raw material (properties are shown in the following Table 1) to carry out hydrocracking reaction in a high pressure reactor, wherein the reaction temperature is 420°C, the initial hydrogen pressure is 10MPa, the catalyst dosage is 500-2000μg / g in terms of metal molybdenum or tungsten, 100-300μg / g in terms of metal nickel, and the reaction time is 1 hour.
[0109] In this test example, the evaluation results of vacuum residue hydrocracking of different oil-soluble catalyst solutions are shown in Table 2 below.
[0110] Table 1 Properties of Middle East high sulfur vacuum residue feedstock
[0111]
[0112]
[0113] Table 2 Distribution of Middle East high sulfur vacuum residue hydrocracking products
[0114]
[0115] It can be seen from the data in Table 2 above that the oil-soluble bimetallic catalyst prepared in the embodiment of the present invention has excellent hydrogenation performance and can effectively inhibit the formation of coke. Under the conditions of reaction temperature of 420°C, initial hydrogen pressure of 10MPa, and reaction time of 1 hour, the metal nickel-modified Y-NW-1 catalyst provided in Example 1 has higher hydrogenation performance than the single tungsten-based catalyst (CW-1) with a dosage of 1870μg / g when the catalyst dosage is 935μg / g (in terms of tungsten) and 300μg / g (in terms of nickel), and the conversion rate (<500°C fraction) can be increased by 4.3 percentage points, and the coke rate is only 0.4wt%.
[0116] It can also be known from the data in Table 2 above that the catalyst (C-NM-3) in Reference Example 2 and the catalyst of Example 3 (Y-NM-1) are not much different in hydrogenation performance, but compared with its preparation process, in Example 3, when preparing the catalyst, the liquid intermediate product ammonium thiomolybdate is first synthesized, and the second metal solution is added to the synthetic liquid intermediate product, and a total of 78.72g of nickel ammonium thiomolybdate is generated through a one-step precipitation, and the yield is 98.4%; and in the preparation process of Reference Example 2, after the intermediate precipitated nickel ammonium molybdate is generated, it is necessary to increase the process of washing, filtering and drying the intermediate precipitated nickel ammonium molybdate, which inevitably causes the loss of part of the metal, the increase of waste water and the growth of the reaction time, and the nickel ammonium thiomolybdate generated by final sulfidation is 77.44g, and the yield is 96.8%, and the product yield is reduced by 1.6 percentage points. It can be seen from this that the preparation method of the catalyst provided in the embodiment of the present invention is simpler and has a higher yield, which is convenient for large-scale industrial production.
[0117] It can also be known from the data in Table 2 above that in the preparation process of the catalyst (C-MN-4) provided in Reference Example 3, the precursor of molybdenum and the precursor of nickel are added to the dispersant catalytic cracking diesel respectively, and Example 3 of the present invention adopts sulfur-containing nickel-molybdenum bimetallic salt complex and organic acid to react to obtain the precursor of sulfur-soluble nickel-molybdenum bimetallic catalyst, and the catalyst is prepared again this time. Compared with C-MN-4, Y-NM-1 provided in Example 3 of the present invention shows better catalyst performance, conversion rate (<500°C fraction) can be increased by 3.2 percentage points, and coking rate is reduced by 0.2wt%. It can be seen that using sulfur-containing nickel-molybdenum bimetallic compound as catalyst precursor is more conducive to the synergistic effect between metallic nickel and molybdenum sulfide, while improving the conversion rate, it can also effectively inhibit coking and reduce the total amount of metal added to the catalyst.
[0118] The above data show that the oil-soluble bimetallic catalyst prepared in the embodiment of the present invention has excellent hydrogenation performance, and is particularly suitable for the slurry bed hydrocracking process of high-metal, high-carbon residue, high-sulfur low-quality heavy oil. The preparation method of the catalyst is simpler and has a higher yield, which is convenient for large-scale industrial production.
[0119] The above is only a specific embodiment of the present invention, and cannot be used to limit the scope of the invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the protection scope of the patent of the present invention, should still fall within the scope of this patent. In addition, the technical features of the present invention can be freely combined with each other, with each other and with each other, and with each other.
Claims
1. A method for preparing an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst, characterized in that: The preparation method comprises: S1: After dissolving a molybdenum source or a tungsten source in ammonia water or water, a sulfiding agent is added to the resulting solution to react with the molybdenum source or the tungsten source to obtain thiomolybdate or thiotungstate; wherein the molar ratio of the sulfur content of the sulfiding agent to molybdenum or tungsten is 2-6:1; the reaction temperature in S1 is 30-150° C., and the reaction time is 0.5-3h; S2: dissolving a nickel source in excess ammonia water, and then mixing the obtained nickel source ammonia solution with the sulfur-containing molybdenum source or sulfur-containing tungsten source solution obtained in S1 to obtain a sulfur-containing nickel-molybdenum bimetallic salt complex or a sulfur-containing nickel-tungsten bimetallic salt complex through reaction; in S2, the reaction temperature is 30-150° C., and the reaction time is 0.5-3 h; S3: reacting a sulfur-containing nickel-molybdenum bimetallic salt complex or a sulfur-containing nickel-tungsten bimetallic salt complex with an organic acid to obtain a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst or a precursor of a nickel-tungsten bimetallic catalyst; S4: dissolving a precursor of an oil-soluble nickel-molybdenum bimetallic catalyst or a precursor of a nickel-tungsten bimetallic catalyst in an organic dispersant to obtain a precursor solution of a nickel-molybdenum bimetallic catalyst or a precursor solution of a nickel-tungsten bimetallic catalyst; S5: dissolving a precursor solution of a nickel-molybdenum bimetallic catalyst or a precursor solution of a nickel-tungsten bimetallic catalyst in a dispersing oil to obtain an oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst.
2. The preparation method according to claim 1, characterized in that: The ratio of the volume of the ammonia water to the mass of the molybdenum source or the tungsten source is 1-2:1, and the units are mL and g, respectively.
3. The preparation method according to claim 1 or 2, characterized in that: The molybdenum source includes one or a combination of molybdenum trioxide, ammonium molybdate, ammonium heptamolybdate tetrahydrate, ammonium metamolybdate, and ammonium paramolybdate.
4. The preparation method according to claim 1 or 2, characterized in that: The tungsten source includes one or a combination of tungsten trioxide, ammonium tungstate, ammonium metatungstate, and ammonium paratungstate.
5. The preparation method according to claim 1 or 2, characterized in that: The sulfiding agent includes one or a combination of ammonium sulfide, sodium sulfide and potassium sulfide.
6. The preparation method according to claim 1, characterized in that: The molar ratio of the ammonia water to the nickel source is 1-10:
1.
7. The preparation method according to claim 1 or 6, characterized in that: The nickel source includes one or more of nickel nitrate, nickel acetate, basic nickel carbonate, nickel sulfate, and nickel formate.
8. The preparation method according to claim 1, characterized in that: The process between S2 and S3 also includes: filtering and washing the product obtained from the reaction in S2, and drying at room temperature to obtain a precipitate, namely, a sulfur-containing nickel-molybdenum bimetallic salt or a sulfur-containing nickel-tungsten bimetallic salt complex.
9. The preparation method according to claim 1, characterized in that: The molar ratio of the organic acid to molybdenum or tungsten is 2-6:
1.
10. The preparation method according to claim 1 or 9, characterized in that: The organic acid includes one or more of alkane acid, cycloalkane acid, oleic acid and linoleic acid.
11. The preparation method according to claim 1 or 9, characterized in that: In S3, the reaction temperature is 50-200°C, and the reaction time is 0.5-5h.
12. The preparation method according to claim 10, characterized in that: In S3, the reaction temperature is 50-200°C, and the reaction time is 0.5-5h.
13. The preparation method according to claim 1, characterized in that: The molar ratio of the organic dispersant to molybdenum or tungsten is 0.1-1:
1.
14. The preparation method according to claim 1 or 13, characterized in that: The organic dispersant comprises one or more of tetralin, decalin, tetrahydrofuran, dimethyl sulfoxide and aniline.
15. The preparation method according to claim 1, characterized in that: The mass ratio of the dispersing oil to the precursor solution of the nickel-molybdenum bimetallic catalyst or the precursor solution of the nickel-tungsten bimetallic catalyst is 1-10:
1.
16. The preparation method according to claim 1 or 15, characterized in that: The dispersant oil includes one or a combination of straight-run gasoline, straight-run diesel, straight-run wax oil, catalytic cracking gasoline, catalytic cracking diesel, catalytic cracking wax oil, catalytic cracking slurry, coker gasoline, coker diesel, coker wax oil, hydrocracking gasoline, hydrocracking diesel, and hydrocracking wax oil.
17. An oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst, characterized in that: The oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst is prepared by the preparation method of the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst according to any one of claims 1 to 16; Wherein, based on the total weight of the catalyst as 100%, the mass percentage of tungsten or molybdenum is 1-20%, and the mass percentage of nickel is 1-12%.
18. Use of the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst according to claim 17 in a slurry bed hydrocracking process for inferior heavy oil.
19. A slurry bed hydrocracking process for inferior heavy oil, characterized in that: The process utilizes the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst described in claim 17 to carry out slurry bed hydrocracking of inferior heavy oil.
20. The process according to claim 19, characterized in that For each gram of inferior heavy oil, the amount of the oil-soluble nickel-tungsten or nickel-molybdenum bimetallic catalyst used is 200-2000 μg in terms of metal molybdenum or tungsten, and 50-1000 μg in terms of metal nickel; The operating conditions of the slurry bed hydrogenation reactor used in the process are: reaction pressure 5-25MPa, reaction temperature 380-450°C, volume space velocity 0.2-1.2h -1 , hydrogen-oil volume ratio 200-1500.