Composite material for detecting H2S gas at low temperature and its preparation and application

Through the heterojunction formation of Sb-doped SnO2 microspheres and g-C3N4 composite materials, the problem of reducing the concentration and mobility of the semiconductor gas sensor at low temperature is solved, and high sensitivity detection of H2S gas is achieved, suitable for low temperatures Deep air detection in the environment.

CN116332226BActive Publication Date: 2024-11-26HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211489280.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-11-26
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

In the low temperature environment of existing semiconductor gas sensors, the carrier concentration and mobility of semiconductor materials are reduced, affecting the high sensitivity detection of H2S gas.

Method used

Sb-doped SnO2 microspheres and g-C3N4 composite materials are used to form heterojunctions through calcination, which improves the separation and transfer efficiency of photogenerated carriers, and is detected under ultraviolet light to enhance gas-sensitive performance.

Benefits of technology

In a low temperature environment (-50℃≤T≤-20℃), high sensitivity detection of H2S gas is achieved, with a fast response speed and is suitable for deep air detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116332226B_ABST
    Figure CN116332226B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of semiconductor oxide technology, and more specifically, relates to a composite material for detecting H2S gas at low temperature, and its preparation and application. The present invention first prepares a precursor of Sb-doped SnO2 microspheres, and then mixes and grinds with g-C3N4 having a mesh structure and calcines to obtain the composite material for low-temperature detection of hydrogen sulfide gas of the present invention. The mesh structure of g-C3N4 has a large surface area, which is easy to wrap the loose porous ATO microspheres. The two are in close contact during the calcination process. The generated ATO@n-CN composite material can form a heterojunction, which can significantly improve the separation and transfer efficiency of photogenerated carriers under the irradiation of ultraviolet light, so that more photogenerated electrons can be generated to combine with physically adsorbed oxygen molecules on the surface of the composite material to form more highly active chemically adsorbed oxygen ions, which can react with more H2S gas to improve gas-sensitive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semiconductor oxides, and more specifically, relates to a composite material for detecting H2S gas at low temperature and a preparation method and application thereof. Background Art

[0002] Kinetic penetration detectors are an important mode and development direction for future extraterrestrial object detection. It refers to the use of pyrotechnics to make the detector drill into a certain depth inside the planet, mainly used for atmosphere, geological environment, water content detection, etc. As a new detection method, it does not affect the main task, and has the advantages of strong expandability (wide detection range), strong adaptability, and high payload mass utilization efficiency. And as a latecomer, its comprehensive detection indicators have reached the international leading level.

[0003] Volatile detection is one of the important exploration tasks of the probe, and its main goal is to measure the types and contents of volatiles (H2O, H2S, NH3, SO2, etc.) in the lunar soil at the lunar south pole. If it is possible to dive into the lunar soil profile and conduct in-situ detection, data such as the comprehensive physical properties of the lunar soil suspected to contain water ice and the distribution law of water ice in the depth profile will be obtained, which can provide the most direct evidence for revealing scientific issues such as the source of water on the moon, the state of occurrence of water, and the abundance of water reserves.

[0004] The most commonly used technology for detecting volatiles in space is the mass spectrometer, but it needs to meet stringent conditions such as small size and high G-value impact resistance for use in penetrating surveyors, which my country is currently unable to develop. It was originally planned to conduct international cooperation with OPEN University in the UK, but it was not implemented for various reasons.

[0005] Semiconductor gas sensors are expected to be used in exploration vehicles due to their high sensitivity, small size and light weight. Since volatile detection faces an extreme low temperature environment, the current semiconductor gas sensors used in low temperature environments (the working environment of exploration missiles is around -20°C) will reduce the carrier concentration and mobility inside the semiconductor material, which will affect the semiconductor material's high sensitivity detection of gas (ppm level). Therefore, it is urgent to develop a semiconductor material for deep space gas detection, so as to realize the detection of volatiles in lunar soil. Summary of the invention

[0006] In view of the defects of the prior art, the purpose of the present invention is to provide a composite material for detecting H2S gas at low temperature and its preparation and application, so as to solve the technical problems that the carrier concentration and mobility inside the semiconductor material are reduced when the hydrogen sulfide gas sensor in the prior art is detected at low temperature, which will affect the high-sensitivity detection of the semiconductor material to the gas.

[0007] To achieve the above object, the present invention provides a method for preparing a composite material for detecting H2S gas at low temperature, comprising the following steps:

[0008] (1) mixing stannous chloride, citric acid and antimony trichloride and dissolving them in a volatile organic solvent, heating them to fully react, cooling them to separate the solid and liquid, washing the separated solid phase to remove impurity ions, and then drying them to obtain a precursor of Sb-doped SnO2 microspheres, which is recorded as ATO microsphere precursor;

[0009] (2) calcining melamine to obtain g-C3N4, denoted as n-CN;

[0010] (3) The ATO microsphere precursor obtained in step (1) and the n-CN obtained in step (2) are mixed and ground until the mixture is uniformly mixed, and then the mixture powder is calcined to obtain an ATO@n-CN composite material.

[0011] Preferably, the molar ratio of stannous chloride, citric acid and antimony trichloride in step (1) is 1:(1-3):(0.01-0.03), and the volatile organic solvent is one or more of ethanol, methanol and N,N-dimethylformamide.

[0012] Preferably, the heating temperature in step (1) is 170-190° C., and the heating time is 10-20 h.

[0013] Preferably, the heating temperature in step (2) is 525-570° C., and the heating time is 1-5 h.

[0014] Preferably, the mass ratio of the n-CN to the ATO microsphere precursor in step (3) is 1 to 10:100, more preferably 2 to 5:100.

[0015] Preferably, the calcination in step (3) has a heating rate of 1 to 3°C / min, a calcination temperature of 500 to 550°C, and a calcination time of 3 to 5h.

[0016] According to another aspect of the present invention, a composite material prepared by the preparation method is provided.

[0017] According to another aspect of the present invention, there is provided an application of the composite material for detecting H2S gas, and more preferably for detecting H2S gas at low temperature.

[0018] Preferably, the composite material detects H2S in an environment at a temperature of T, wherein -50°C ≤ T ≤ -20°C.

[0019] Preferably, the composite material is subjected to detection of H2S gas at low temperature under ultraviolet light, wherein the wavelength of the ultraviolet light is further preferably 365±5nm and the light intensity is 0.5-0.8mW / cm 2 .

[0020] According to another aspect of the present invention, a H2S gas detection sensor is provided, using the composite material as the sensitive material of the sensor.

[0021] In general, the above technical solution conceived by the present invention has the following advantages compared with the prior art:

[0022] Beneficial effects:

[0023] (1) The present invention first prepares a precursor of Sb-doped SnO2 microspheres, and then mixes and grinds the precursor with g-C3N4 having a mesh structure and then calcines the precursor to obtain the composite material for low-temperature detection of hydrogen sulfide gas of the present invention. The mesh structure of g-C3N4 has a large surface area, which can easily wrap the loose porous ATO microspheres. During the calcination process, the two are in close contact, and the generated ATO@n-CN composite material can form a heterojunction. Under the irradiation of ultraviolet light, the separation and transfer efficiency of photogenerated carriers can be significantly improved, so that more photogenerated electrons can be generated to combine with physically adsorbed oxygen molecules on the surface of the composite material to form more highly active chemically adsorbed oxygen ions, which can react with more H2S gas to improve the gas sensing performance.

[0024] (2) The composite material provided by the present invention can be used to detect H2S gas in a low temperature environment (-50°C ≤ T ≤ -20°C), and has a fast response speed and extremely high sensitivity. In a preferred embodiment, the response value of the composite material to 2 ppm of H2S gas reaches 20.1. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a morphology diagram of the ATO prepared in Comparative Example 2 of the present invention.

[0026] Figure 2 This is a morphology picture of ATO@4n-CN prepared in Example 2 of the present invention.

[0027] Figure 3 This is a graph showing the gas-sensitive response recovery curves of pure SnO2 and ATO generated in Comparative Examples 1 and 2 of the present invention, and ATO@2n-CN, ATO@4n-CN, ATO@6n-CN, and ATO@8n-CN generated in Examples 1 to 4 to H2S under ultraviolet light irradiation at -20°C.

[0028] Figure 4 This is the gas-sensitive response diagram of pure SnO2 prepared in Comparative Example 1 to H2S without ultraviolet irradiation.

[0029] Figure 5 This is the gas-sensitive response diagram of ATO@4n-CN prepared in Example 2 of the present invention to H2S under conditions without ultraviolet irradiation.

[0030] Figure 6 : is a SEM image of pure SnO2 (EDTA as a chelating agent) prepared in Comparative Example 4 of the present invention.

[0031] Figure 7 : is a SEM image of pure SnO2 (EDTA-2Na as a chelating agent) prepared in Comparative Example 5 of the present invention.

[0032] Figure 8 This is the SEM image of pure SnO2 (citric acid as a chelating agent) prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0034] The present invention provides a method for preparing a composite material for detecting H2S gas at low temperature, comprising the following steps:

[0035] (1) mixing stannous chloride, citric acid and antimony trichloride and dissolving them in a volatile organic solvent, heating them to fully react, cooling them to separate the solid and liquid, washing the solid phase to remove impurity ions, and then drying them to obtain a precursor of Sb-doped SnO2 microspheres, which is recorded as ATO microsphere precursor;

[0036] (2) calcining melamine to obtain g-C3N4, denoted as n-CN;

[0037] (3) The ATO microsphere precursor obtained in step (1) and the n-CN obtained in step (2) are mixed and ground until the mixture is uniformly mixed, and then the mixture powder is calcined to obtain an ATO@n-CN composite material.

[0038] In some embodiments, the molar ratio of stannous chloride, citric acid and antimony trichloride in step (1) is 1: (1-3): (0.01-0.03), and the volatile organic solvent is one or more of ethanol, methanol and N,N-dimethylformamide. The heating temperature in step (1) is 170-190°C, and the heating time is 10-20h. Stannous chloride can be stannous chloride dihydrate, and citric acid can be citric acid monohydrate. Citric acid is used as a chelating agent here, and other chelating agents such as EDTA or EDTA-2Na are also tried in the experiment, but the experiment found that the ATO precursor material prepared by using other chelating agents under the same conditions has serious agglomeration phenomenon, and porous ATO precursor microspheres cannot be obtained.

[0039] In some embodiments, the heating temperature in step (2) is 525-570° C. and the heating time is 1-5 hours. Melamine is heated and calcined to obtain blocky g-C3N4, which is denoted as n-CN.

[0040] In some embodiments, the mass ratio of n-CN to the ATO microsphere precursor in step (3) is 1 to 10:100, preferably 2 to 5:100. The heating rate of the calcination in step (3) is 1 to 3°C / min, the calcination temperature is 500 to 550°C, and the calcination time is 3 to 5h.

[0041] Since the detection of volatiles faces an extreme low-temperature environment, the semiconductor gas sensor currently used in the low-temperature environment (the working environment of the reconnaissance bomb is about -20°C) has very little external energy obtained by the electrons in the transition process, resulting in only a few electrons being able to transition to the conduction band of SnO2, thereby reducing the carrier concentration and mobility inside the semiconductor material, which will affect the semiconductor material's high-sensitivity detection of gas (ppm level). The present invention first prepares a precursor of Sb-doped SnO2 microspheres, denoted as ATO microsphere precursor, and by selecting a suitable chelating agent citric acid, the prepared ATO microsphere precursor has a porous structure, and then is mixed with g-C3N4 having a mesh structure, ground and calcined to obtain the composite material. The composite material prepared by the above-mentioned preparation method of the present invention includes a mesh structure n-CN and ATO microspheres coated inside the mesh structure n-CN. The morphology of n-CN in the composite material is a mesh structure, and the morphology of ATO microspheres in the composite material is a loose and porous microsphere structure; and the pores of the mesh structure n-CN are larger than the pore size of the ATO microspheres. Therefore, when the composite material is used to detect H2S gas at low temperature, the gas can pass through the n-CN and the ATO microspheres in sequence and enter the interior of the composite material. In addition, the porous structure is also conducive to the ultraviolet light entering the interior of the composite material, interacting with the sensitive material to increase the concentration of photogenerated carriers.

[0042] The composite material prepared by the present invention has been proven to be able to be used for high-sensitivity detection of H2S gas at low temperatures. First, an ATO microsphere precursor with a porous structure is prepared by selecting a suitable chelating agent to react with an antimony salt and a tin salt, and at the same time, due to the addition of antimony into the ATO microsphere precursor, the conductivity of the composite material is improved, its resistance is reduced, and the charge transfer efficiency is improved. The present invention further grinds and calcines the ATO microsphere precursor with a photocatalyst mesh g-C3N4, and the addition of the mesh photocatalyst calcination can make the two composite to form a heterojunction, improve the separation and transmission efficiency of photogenerated carriers, and form more highly active photogenerated chemically adsorbed oxygen ions, thereby greatly enhancing the gas-sensitive activity at low temperatures; further, the present invention uses the composite material for detecting H2S at low temperatures, and detects it under ultraviolet light. Experiments have found that ultraviolet light can further increase the concentration of photogenerated carriers and improve gas sensitivity. In some embodiments, the composite material can detect H2S in an environment with a temperature of T, wherein -50°C≤T≤-20°C. The composite material is subjected to detection of H2S gas at low temperature under ultraviolet light irradiation, wherein the wavelength of the ultraviolet light is 365±5nm and the light intensity is 0.5-0.8mW / cm 2 .

[0043] The preparation method of the composite material in the embodiment of the present invention is described in detail below:

[0044] Example 1

[0045] This embodiment describes in detail a composite material for detecting H2S gas at low temperature and a preparation method thereof, which includes the following steps:

[0046] S1. Preparation of ATO microsphere precursor: 0.01 mol of stannous chloride dihydrate, 0.02 mol of citric acid monohydrate and 0.0002 mol of antimony trichloride were added to 50 mL of anhydrous ethanol and stirred magnetically for 0.5 h. The mixed solution was then transferred to a 100 mL hydrothermal reactor and reacted at 180 ° C for 12 h. After natural cooling, the generated powder was centrifuged and washed with water and ethanol for 3 times respectively, and then placed in an oven at 100 ° C for 12 h to obtain a precursor of Sb-doped SnO2 microspheres, which was marked as ATO microsphere precursor;

[0047] S2. Preparation of bulk g-C3N4: 5 g of melamine was placed in a half-covered crucible and calcined at 550 °C for 2 h to obtain bulk g-C3N4;

[0048] S3. Preparation of ATO@2n-CN: The ATO microsphere precursor generated in step S1 is transferred to an agate mortar, and then the bulk g-C3N4 generated in step S2 is added, the mass of the bulk g-C3N4 is 2% of the mass of the ATO microsphere precursor, and the two are fully ground until they are evenly mixed; the mixture powder is placed in a porcelain boat and kept flat, the porcelain boat is placed in a muffle furnace, the temperature is raised to 525°C and calcined for 4 hours, the heating rate is controlled at 2°C / min, and after cooling to room temperature, a composite material is obtained, which is marked as ATO@2n-CN.

[0049] Example 2

[0050] This embodiment describes in detail a composite material for detecting H2S gas at low temperature and a preparation method thereof, which includes the following steps:

[0051] S1. Preparation of ATO microsphere precursor: 0.01 mol of stannous chloride dihydrate, 0.02 mol of citric acid monohydrate and 0.0002 mol of antimony trichloride were added to 50 mL of anhydrous ethanol and stirred magnetically for 0.5 h. The mixed solution was then transferred to a 100 mL hydrothermal reactor and reacted at 180 ° C for 12 h. After natural cooling, the generated powder was centrifuged and washed with water and ethanol for 3 times respectively, and then placed in an oven at 100 ° C for 12 h to obtain a precursor of Sb-doped SnO2 microspheres, which was marked as ATO microsphere precursor;

[0052] S2. Preparation of bulk g-C3N4: 5 g of melamine was placed in a half-covered crucible and calcined at 550 °C for 2 h to obtain bulk g-C3N4;

[0053] S3. Preparation of ATO@4n-CN: The ATO microsphere precursor generated in step S1 is transferred to an agate mortar, and then the bulk g-C3N4 generated in step S2 is added, the mass of the bulk g-C3N4 is 4% of the mass of the ATO microsphere precursor, and the two are fully ground until they are evenly mixed; the mixture powder is placed in a porcelain boat and kept flat, the porcelain boat is placed in a muffle furnace, the temperature is raised to 525°C and calcined for 4 hours, the heating rate is controlled at 2°C / min, and a composite material is obtained after cooling to room temperature, which is marked as ATO@4n-CN.

[0054] Example 3

[0055] This embodiment describes in detail a composite material for detecting H2S gas at low temperature and a preparation method thereof, which includes the following steps:

[0056] S1. Preparation of ATO microsphere precursor: 0.01 mol of stannous chloride dihydrate, 0.02 mol of citric acid monohydrate and 0.0002 mol of antimony trichloride were added to 50 mL of anhydrous ethanol and stirred magnetically for 0.5 h. The mixed solution was then transferred to a 100 mL hydrothermal reactor and reacted at 180 ° C for 12 h. After natural cooling, the generated powder was centrifuged and washed with water and ethanol for 3 times respectively, and then placed in an oven at 100 ° C for 12 h to obtain a precursor of Sb-doped SnO2 microspheres, which was marked as ATO microsphere precursor;

[0057] S2. Preparation of bulk g-C3N4: 5 g of melamine was placed in a half-covered crucible and calcined at 550 °C for 2 h to obtain bulk g-C3N4;

[0058] S3. Preparation of ATO@6n-CN: The ATO microsphere precursor generated in step S1 is transferred to an agate mortar, and then the bulk g-C3N4 generated in step S2 is added, the mass of the bulk g-C3N4 is 6% of the mass of the ATO microsphere precursor, and the two are fully ground until they are evenly mixed; the mixture powder is placed in a porcelain boat and kept flat, the porcelain boat is placed in a muffle furnace, the temperature is raised to 525°C and calcined for 4 hours, the heating rate is controlled at 2°C / min, and after cooling to room temperature, a composite material is obtained, which is marked as ATO@6n-CN.

[0059] Example 4

[0060] This embodiment describes in detail a composite material for detecting H2S gas at low temperature and a preparation method thereof, which includes the following steps:

[0061] S1. Preparation of ATO microsphere precursor: 0.01 mol of stannous chloride dihydrate, 0.02 mol of citric acid monohydrate and 0.0002 mol of antimony trichloride were added to 50 mL of anhydrous ethanol and stirred magnetically for 0.5 h. The mixed solution was then transferred to a 100 mL hydrothermal reactor and reacted at 180 ° C for 12 h. After natural cooling, the generated powder was centrifuged and washed with water and ethanol for 3 times respectively, and then placed in an oven at 100 ° C for 12 h to obtain a precursor of Sb-doped SnO2 microspheres, which was marked as ATO microsphere precursor;

[0062] S2. Preparation of bulk g-C3N4: 5 g of melamine was placed in a half-covered crucible and calcined at 550 °C for 2 h to obtain bulk g-C3N4;

[0063] S3. Preparation of ATO@8n-CN: The ATO microsphere precursor generated in step S1 is transferred to an agate mortar, and then the bulk g-C3N4 generated in step S2 is added, the mass of the bulk g-C3N4 is 8% of the mass of the ATO microsphere precursor, and the two are fully ground until they are evenly mixed; the mixture powder is placed in a porcelain boat and kept flat, the porcelain boat is placed in a muffle furnace, the temperature is raised to 525°C and calcined for 4 hours, the heating rate is controlled at 2°C / min, and a composite material is obtained after cooling to room temperature, which is marked as ATO@8n-CN.

[0064] Comparative Example 1

[0065] This comparative example describes in detail an oxide semiconductor for detecting H2S gas at low temperature and a preparation method thereof, comprising the following steps:

[0066] Preparation of pure SnO2: weigh 0.01 mol SnCl2·2H2O and 0.02 mol C6H 10 O8·H2O and beaker, add 50mL of anhydrous ethanol, stir magnetically for 0.5h, then transfer the mixed solution to a 100mL hydrothermal reactor, react at 180℃ for 12h, and after natural cooling, centrifuge and wash the generated powder with water and ethanol for 3 times respectively, then dry it in an oven at 100℃ for 12h, finally transfer the powder to a porcelain boat and calcine it in a muffle furnace at a calcination temperature of 525℃, a calcination time of 2h, a heating rate of 5℃ / min, and a cooling rate of 1℃ / min to finally obtain SnO2 powder monomer.

[0067] Comparative Example 2

[0068] This embodiment describes in detail an oxide semiconductor for detecting H2S gas at low temperature and a preparation method thereof, including the following steps:

[0069] Preparation of ATO microspheres: 0.01 mol of stannous chloride dihydrate, 0.02 mol of citric acid monohydrate and 0.0002 mol of antimony trichloride were added to 50 mL of anhydrous ethanol and magnetically stirred for 0.5 h. The mixed solution was then transferred to a 100 mL hydrothermal reactor and reacted at 180 ° C for 12 h. After natural cooling, the generated powder was centrifuged and washed with water and ethanol for 3 times respectively, and then placed in an oven at 100 ° C for 12 h. Finally, the powder was transferred to a porcelain boat and calcined in a muffle furnace at a calcination temperature of 525 ° C, a calcination time of 2 h, a heating rate of 5 ° C / min, and a cooling rate of 1 ° C / min to finally obtain ATO microspheres.

[0070] like Figure 1 As shown, it is a morphology diagram of ATO generated in Comparative Example 2 of the present invention. It can be seen that the morphology of the material is a loose and porous spherical structure;

[0071] like Figure 2 As shown in the figure, it is a morphology of ATO@4n-CN generated in Example 2 of the present invention. It can be seen that the morphology of the material is a mesh g-C3N4 wrapped loose porous ATO microsphere structure; this mesh structure of g-C3N4 has a large surface area and can easily wrap the loose porous ATO microspheres. The two materials are in close contact during the calcination process, and the generated mesh g-C3N4 flakes can wrap the ATO microspheres to the greatest extent and form a composite material.

[0072] The application of the composite material in the embodiment of the present invention for detecting H2S gas at low temperature is described in detail below:

[0073] ATO@xn-CN composite materials with different n-CN contents were used as sensitive materials (specifically including ATO@2n-CN prepared in Example 1, ATO@4n-CN prepared in Example 2, ATO@6n-CN prepared in Example 3, and ATO@8n-CN prepared in Example 4) to make gas sensors, which were placed in a test chamber at -20°C and irradiated with ultraviolet light for testing. The specific preparation method is as follows: The gas sensor was prepared by drip coating. First, 20 mg of the composite material of the above example was weighed and transferred to a centrifuge tube, and then 1 mL of anhydrous ethanol was added. The centrifuge tube was placed in an ultrasonic cleaner for 10 minutes. When the composite material is evenly dispersed, 0.1 mL of the dispersion was immediately drawn with a syringe and evenly dripped onto a ceramic sheet pre-printed with gold interdigital electrodes, and allowed to stand for 0.5 hours to form a film, and finally a H2S gas sensor was obtained.

[0074] The low temperature test system consists of a three-layer Dewar flask structure. The innermost layer is a test chamber with a volume of 1L. A PT100 temperature sensor is placed near the gas sensor in the test chamber. In order to ensure the airtightness of the chamber, the temperature sensor is connected to the external display through an aviation plug so that the temperature in the test chamber can be read and controlled at any time. The two test probes in the test chamber are also connected to the external Keithley 6487 picoammeter through an aviation plug, and the picoammeter is connected to the test computer. A UV LED lamp with a wavelength of 365nm and a light intensity of 0.65mW / cm is installed directly above the sensor. 2, the LED lamp is powered by an external power supply and is also connected through an aviation plug. The middle layer is a cooling chamber, which is used to cool the test cavity. The temperature of the test chamber is controlled by injecting an appropriate amount of liquid nitrogen into the cooling chamber and observing the display of the temperature sensor. The outermost layer is a vacuum insulation layer, which is used to isolate the cooling chamber from the external environment to prevent the rapid volatilization of liquid nitrogen, thereby affecting the cooling and insulation effects. Before the test, the humid air in the test chamber needs to be replaced with dry air to prevent the test cavity and the parts in the cavity from frosting in a low temperature environment, which will affect the test of the gas sensor. During the entire UV photocatalytic promotion of low-temperature gas performance test process, the UV lamp has been turned on. When studying the response process of the gas sensor, open the air inlet valve, then inject the target gas into the top rubber plug through a syringe, inject a certain concentration of gas into the test cavity, and the gas sensor responds. When studying the recovery process of the gas sensor, open the air outlet valve, then use a vacuum pump to extract the gas in the cavity, and inject dry air at the same time, and the gas sensor recovers.

[0075] like Figure 3 As shown, it is a gas-sensitive response recovery curve of pure SnO2 and ATO generated in Comparative Examples 1 and 2 of the present invention, and ATO@2n-CN, ATO@4n-CN, ATO@6n-CN, ATO@8n-CN generated in Examples 1 to 4 to H2S under -20°C ultraviolet light irradiation. When 2ppm H2S gas is injected, the response value of the pure SnO2 gas sensor is only 2.1, the response time is as long as 66s, and the recovery process requires a longer time. The response value of the ATO gas sensor corresponding to Comparative Example 2 under ultraviolet light irradiation is 2.4, slightly higher than pure SnO2, and the response time is 82 seconds. The experimental results show that the gas-sensitive performance of pure SnO2 gas sensors and ATO gas sensors under ultraviolet light irradiation is poor.

[0076] ATO@xn-CN composites may form a heterojunction, which can significantly improve the separation and transfer efficiency of photogenerated carriers under ultraviolet light irradiation. Therefore, more photogenerated electrons can be generated to combine with physically adsorbed oxygen molecules on the surface of the composite material to form more highly active chemically adsorbed oxygen ions, which can react with more H2S gas to improve the gas sensing performance. By comparing ATO@4n-CN and ATO@2n-CN, it is found that the response speed of ATO@4n-CN (response time: 14s) is significantly higher than that of ATO@2n-CN (response time: 55s), and the response value is 20.1, which is also much higher than ATO@2n-CN. The initial resistance of ATO@6n-CN and ATO@8n-CN gas sensors is very high, which may be due to the excessive amount of composite n-CN. In addition, the vibration of its resistance change curve is very strong, so the response value is low, the response recovery time is long, and the gas sensing performance is poor. Therefore, the embodiment of the present invention can obtain a suitable initial resistance by compounding ATO with an appropriate amount of n-CN, and the formation of a heterojunction can significantly improve the separation and transfer efficiency of carriers, which is helpful to improve the gas sensing performance, and is therefore suitable for detecting H2S gas at low temperatures.

[0077] As a control, the above test system was also used to test the gas sensing properties of pure SnO2 powder and the ATO@4n-CN composite material prepared in Example 2 under dark conditions (i.e., without ultraviolet irradiation) in the same way during the experiment. The results are as follows: Figure 4 and Figure 5 As shown, it can be seen that pure SnO2 and ATO@4n-CN composites are insensitive to H2S gas without UV irradiation.

[0078] Comparative Example 3

[0079] This comparative example describes in detail an oxide semiconductor for detecting H2S gas at low temperature and a preparation method thereof, comprising the following steps:

[0080] Preparation of In-doped SnO2 microspheres: 0.01 mol of stannous chloride dihydrate, 0.02 mol of citric acid monohydrate and 0.0002 mol of indium trichloride were added to 50 mL of anhydrous ethanol and magnetically stirred for 0.5 h. The mixed solution was then transferred to a 100 mL hydrothermal reactor and reacted at 180 ° C for 12 h. After natural cooling, the resulting powder was centrifuged and washed with water and ethanol for 3 times respectively, and then placed in an oven at 100 ° C for 12 h. Finally, the powder was transferred to a porcelain boat and calcined in a muffle furnace at a calcination temperature of 525 ° C, a calcination time of 2 h, a heating rate of 5 ° C / min, and a cooling rate of 1 ° C / min to finally obtain In-doped SnO2 microspheres. In-doped SnO2 microspheres were used to detect H2S gas at room temperature using the above method, and the experiment found no response; while under the same conditions, the prepared Sb-doped SnO2 microspheres were used to detect H2S gas at room temperature using the above method, and had a better response. Therefore, in the experiments of the present invention, Sb doping was used to prepare composite materials for low-temperature detection of H2S gas.

[0081] Comparative Example 4

[0082] This comparative example investigates the use of EDTA as a chelating agent to prepare tin dioxide powder, comprising the following steps:

[0083] Preparation of pure SnO2 (EDTA): Weigh 0.01mol SnCl2·2H2O and 0.02mol EDTA in a beaker, add 50mL anhydrous ethanol, stir magnetically for 0.5h, then transfer the mixed solution to a 100mL hydrothermal reactor, react at 180℃ for 12h, and after natural cooling, centrifuge and wash the generated powder with water and ethanol for 3 times, then place it in an oven at 100℃ for 12h, finally transfer the powder to a porcelain boat, put it in a muffle furnace for calcination, the calcination temperature is 525℃, the calcination time is 2h, the heating rate is 5℃ / min, the cooling rate is 1℃ / min, and finally obtain SnO2 powder monomer. The SnO2 grains are severely agglomerated and have a non-porous structure, so it is not conducive to the diffusion of gas between materials.

[0084] Comparative Example 5

[0085] This comparative example investigates the use of EDTA-2Na as a chelating agent to prepare tin dioxide powder, comprising the following steps:

[0086] Preparation of pure SnO2 (EDTA-2Na): Weigh 0.01mol SnCl2·2H2O and 0.02mol EDTA-2Na respectively in a beaker, add 50mL anhydrous ethanol, stir magnetically for 0.5h, then transfer the mixed solution to a 100mL hydrothermal reactor, react at 180℃ for 12h, and after natural cooling, centrifuge and wash the generated powder with water and ethanol for 3 times, then place it in an oven at 100℃ for 12h, finally transfer the powder to a porcelain boat, put it in a muffle furnace for calcination, the calcination temperature is 525℃, the calcination time is 2h, the heating rate is 5℃ / min, the cooling rate is 1℃ / min, and finally obtain SnO2 powder monomer. The SnO2 grains are severely agglomerated and have a non-porous structure, so it is not conducive to the diffusion of gas between materials.

[0087] Example 5

[0088] This example investigates the use of citric acid as a chelating agent to prepare tin dioxide powder, comprising the following steps:

[0089] Preparation of pure SnO2 (EDTA-2Na): Weigh 0.01mol SnCl2·2H2O and 0.02mol citric acid in a beaker, add 50mL anhydrous ethanol, stir magnetically for 0.5h, then transfer the mixed solution to a 100mL hydrothermal reactor, react at 180℃ for 12h, and after natural cooling, centrifuge and wash the generated powder with water and ethanol for 3 times, then place it in an oven at 100℃ for 12h, finally transfer the powder to a porcelain boat, put it in a muffle furnace for calcination, the calcination temperature is 525℃, the calcination time is 2h, the heating rate is 5℃ / min, and the cooling rate is 1℃ / min, finally obtaining SnO2 powder. The SnO2 grains are porous microspheres, which are conducive to the diffusion of gas between materials.

[0090] Figure 6 , Figure 7 and Figure 8 The morphology pictures of pure tin dioxide powder prepared by different chelating agents are shown in Comparative Example 4, Comparative Example 5 and Example 5 respectively. It can be seen that when EDTA or EDTA-2Na is used as the chelating agent, the prepared SnO2 powder is severely agglomerated, and porous microspherical tin dioxide powder can only be obtained when citric acid is used. Therefore, the other embodiments of the present invention use citric acid as the chelating agent to further synthesize antimony-doped ATO porous microsphere precursor.

[0091] The above are only preferred embodiments of the present invention and are not intended to limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention according to the drawings and the above embodiments. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a composite material for detecting H2S gas at low temperature, characterized in that: The steps include: (1) Stannous chloride, citric acid and antimony trichloride are mixed and dissolved in a volatile organic solvent, heated to fully react, cooled and then separated into solid and liquid, washed the separated solid phase to remove impurity ions, and then dried to obtain a precursor of Sb-doped SnO2 microspheres, which is recorded as ATO microsphere precursor; the volatile organic solvent is one or more of ethanol, methanol and N,N-dimethylformamide; the heating temperature is 170-190°C, and the heating time is 10-20 h; (2) Calcination of melamine to obtain g-C3N4, denoted as n-CN; (3) The ATO microsphere precursor obtained in step (1) and the n-CN obtained in step (2) are mixed and ground until they are uniformly mixed, and then the mixture powder is calcined to obtain an ATO@n-CN composite material; the mass ratio of the n-CN to the ATO microsphere precursor is 2 to 4:

100.

2. The preparation method according to claim 1, characterized in that The molar ratio of stannous chloride, citric acid and antimony trichloride in step (1) is 1:(1-3):(0.01-0.03).

3. The preparation method according to claim 1, characterized in that: The calcination temperature in step (2) is 525-570° C. and the heating time is 1-5 h.

4. The preparation method according to claim 1, characterized in that: The calcination in step (3) has a heating rate of 1-3°C / min, a calcination temperature of 500-550°C, and a calcination time of 3-5h.

5. The composite material prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the composite material according to claim 5, characterized in that: Used to detect H2S gas.

7. The use according to claim 6, characterized in that Used to detect H2S gas at low temperatures.

8. The use according to claim 6, characterized in that The composite material detects H2S in an environment with a temperature of T, wherein -50°C≤T≤-20°C.

9. The use according to claim 8, characterized in that The composite material is subjected to detection of H2S gas at low temperature under ultraviolet light irradiation, wherein the wavelength of the ultraviolet light is 365±5nm and the light intensity is 0.5-0.8 mW / cm 2 .

10. A H2S gas detection sensor, characterized in that: The composite material as claimed in claim 5 is used as the sensitive material of the sensor.