A low yield strength ratio bridge steel plate and its manufacturing method

Through specific chemical composition and manufacturing processes, low yield strength ratio bridge steel plates with ferrite + granular bainite structure were prepared, which solved the problem of excessive yield strength ratio of bridge steel and achieved a balance between high strength and low yield strength ratio. , improves the safety and weather resistance of bridge steel.

CN116334478BActive Publication Date: 2024-11-15JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310073641.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-07
Publication Date
2024-11-15
Estimated Expiration
2043-02-07

AI Technical Summary

Technical Problem

Under the high strength requirements, the yield ratio of existing bridge steel is too high, resulting in poor safety and difficult to meet the application needs of high-strength bridge projects.

Method used

Through specific chemical composition combinations and manufacturing processes, including controlled rolling and cooling processes and step cooling processes, low yield strength ratio bridge steel plates with ferrite + granular bainite structure are prepared, with chemical composition of C0.04-0.07%. Si0.25-0.40%, Mn1.60-1.80%, Al0.02-0.04%, Nb0.045-0.055%, Ti0.01-0.02%, Cr0.10-0.30%, Ni0.10-0.30%, Cu0 .10-0.30%, Mo0.10-0.30%, and adopts a three-stage step slow cooling process and online hooded stack slow cooling treatment.

Benefits of technology

It achieves the reduction of yield and strength ratio while ensuring strength while ensuring strength, improves the low-temperature toughness and elongation of the steel plate, and ensures the safety and weather resistance of bridge steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116334478B_ABST
    Figure CN116334478B_ABST
Patent Text Reader

Abstract

The invention relates to a low yield strength ratio bridge steel plate and a manufacturing method thereof. The chemical composition (wt.%) is C0.04-0.07; Si 0.25-0.40; Mn 1.60-1.80; Alt 0.02-0.04; Nb 0.045-0.055; Ti 0.01-0.02; Cr0.10-0.30; Ni 0.10-0.30; Cu 0.10-0.30; Mo 0.10-0.30; the balance is Fe and inevitable impurities. The manufacturing method comprises the following steps: converter smelting, LF+RH refining, slab continuous casting, slab heating, controlled rolling and controlled cooling, etc., and can obtain a ferrite+granular bainite structure with a yield strength of ≥500MPa, a tensile strength of ≥700MPa, a yield strength ratio of ≤0.80, an elongation of ≥30%, and an impact energy of ≥200J at -40°C, thereby ensuring that the strength meets the requirements and having a low yield strength ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of special steel smelting, and specifically relates to a low yield ratio bridge steel plate and a manufacturing method thereof. Background Art

[0002] With the continuous improvement of my country's infrastructure, more and more large-scale bridges with large spans, heavy loads and highly complex geological conditions are being built, which puts forward urgent requirements for high-strength and lightweight bridge steel. In the process of high-strength and lightweight bridge steel, the yield strength ratio of traditional materials continues to increase with the increase of yield strength. As an important indicator for measuring the fracture safety of materials, the larger the value of the yield strength ratio, the worse the safety, which has become a technical bottleneck restricting the application of high-strength bridge steel engineering. How to solve the problem of the yield strength ratio of high-strength bridge steel, while ensuring that the strength meets the requirements, has a lower yield strength ratio, has become the latest research and development hotspot.

[0003] Patent announcement number CN 111455287A proposes a 500MPa grade low yield ratio weathering bridge steel and its manufacturing method. Through the manufacturing method of controlled rolling and controlled cooling + tempering, the characteristics of low yield ratio, high and low temperature toughness and high ductility are obtained. Because it requires weather resistance, a large amount of Cu, Ni, Cr and other elements are used in the composition design. Compared with this patent, there are obvious differences in the composition system and process route. Patent announcement number CN 113186454 A proposes a production method for tempered low yield ratio bridge steel. The process of controlled rolling and controlled cooling + offline tempering is used to obtain a low yield ratio bridge steel plate. Compared with this patent, there are obvious differences in the range of key alloy elements, the final cooling temperature range and the offline heat treatment process. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a low yield strength ratio bridge steel plate and a manufacturing method thereof in view of the above-mentioned prior art, which has a lower yield strength ratio while ensuring that the strength meets the requirements.

[0005] The technical solution adopted by the present invention to solve the above-mentioned problem is: a low yield strength ratio bridge steel plate, characterized in that the chemical composition of the steel includes, by mass percentage, the following: C 0.04-0.07; Si 0.25-0.40; Mn 1.60-1.80; Alt 0.02-0.04; Nb 0.045-0.055; Ti 0.01-0.02; Cr 0.10-0.30; Ni 0.10-0.30; Cu 0.10-0.30; Mo 0.10-0.30; the balance is Fe and unavoidable impurities.

[0006] The steel plate has a yield strength of ≥500MPa, a tensile strength of ≥700MPa, a yield strength ratio of ≤0.80, an elongation of ≥30%, and an impact energy of ≥200J at -40°C.

[0007] The steel plate is produced by a controlled rolling and controlled cooling process to obtain a ferrite+granular bainite structure.

[0008] The functions of all key components contained in the present invention and the reasons for selecting their contents are specifically described as follows:

[0009] C: A key factor affecting phase transformation and low-temperature toughness in steel. When the content is too high, the center segregation will increase, resulting in a decrease in low-temperature toughness. At the same time, it is easy to obtain ferrite + pearlite structure with poor low-temperature toughness. If the content is too low, the strengthening effect is insufficient. In this patent, the C content is selected in the range of 0.04-0.07% to comprehensively balance the low-temperature toughness, weldability and granular bainite structure transformation characteristics.

[0010] Si: a main deoxidizing element, having a solid solution strengthening effect. The Si content in the present invention is selected within a range of 0.25-0.40%.

[0011] Mn: Main alloy strengthening element, improves the strength and toughness of steel in the form of solid solution strengthening, which is beneficial to the control of yield ratio; too high a content is harmful to weldability. The present invention considers the combined effects of carbon and manganese on weldability and low-temperature toughness, and under the premise of low-carbon design, the reasonable selection range of Mn is 1.60-1.80%.

[0012] Alt: a major deoxidizing element and a grain-refining element, and plays a role in grain refinement by forming AltN. The content of Alt in the present invention is selected within a range of 0.02-0.04%.

[0013] Nb: the most important grain-refining element, which can significantly increase the austenite recrystallization temperature of steel, expand the range of the non-recrystallization zone, and refine the original austenite grain size; when rolling in the non-recrystallization zone, fine Nb (C, N) precipitation phase is formed to refine the ferrite grains; from the perspective of fully refining the grains to ensure strength, the present invention selects a range of 0.045-0.055%.

[0014] Ti: fine grains, used in combination with Nb, can reduce the probability of surface star cracks. At the same time, TiN refines the grain size of the heat affected zone of welding and improves the low temperature toughness of the heat affected zone of welding. Taking all factors into consideration, the selection range of Ti is 0.01-0.02%.

[0015] Cr: It can form a continuous solid solution, reduce the austenite phase area, increase the hardenability of steel, and improve the strength of carbon steel. Too high a Cr content will reduce the cross-sectional shrinkage and impact toughness of steel. In the present invention, the influence on hardenability is comprehensively considered, and the Cr content is selected in the range of 0.10-0.30%.

[0016] Mo: It can delay the ferrite phase transformation, improve the hardenability of steel, prevent temper brittleness, and be conducive to obtaining bainite structure at a lower cooling rate. In the present invention, the influence of Mo on the phase transformation is fully utilized, combined with precise cooling process settings, to obtain the designed structure and performance. Taking comprehensive considerations, the Mo content is selected in the range of 0.10-0.30%.

[0017] Ni: Nickel is infinitely solid-dissolved with iron, which has a good effect on improving strength and low-temperature toughness, while reducing the critical transformation rate and improving hardenability. In the present invention, the contribution of Ni element to strength and toughness is mainly utilized, and the selection range is 0.10-0.30%;

[0018] Cu: Copper in bridge steel can improve the atmospheric corrosion resistance of steel and also contribute to strength; too high copper content is prone to cause thermal cracks, so Cu content is used in combination with Ni. In the present invention, the Cu content selection range is 0.10-0.30%.

[0019] The present invention also provides a method for manufacturing a low yield strength ratio bridge steel plate, comprising the following process steps: smelting raw materials in turn through top and bottom blowing in a converter, LF+RH refining, and continuous casting to obtain a 150 / 370mm thick continuous casting billet; 150mm heating furnace in the furnace time 180-210min, 370mm in the furnace time 400-430min, soaking section insulation temperature 1180-1200℃, insulation time ≥40min; rolling stage adopts a large compression ratio rolling process, the total compression ratio ≥10, and the The compression ratio in the medium and rough rolling stage is ≥4 times, the starting rolling temperature is 1050-1170℃, and the average reduction rate of the last three passes is ≥20%; the compression ratio in the finishing rolling stage is ≥3 times, the starting rolling temperature is 800-860℃, and the final rolling temperature is 780-820℃; after rolling, the steel plate is subjected to a step cooling process design, air cooling within ≤30s after rolling, weak cooling within 30-50s, the cooling rate range is set to 4-6℃ / s, and the cooling intensity is increased after >50s, the cooling rate range is set to 5-8℃ / s, and the final cooling temperature is 400-450℃. The cooling rate is accurately set by step to obtain the medium-temperature transformation structure of ferrite + granular bainite structure; after cooling, the steel plate is quickly unloaded and slowly cooled with a cover pile, the unload temperature is ≥350℃, and the pile slow cooling time is ≥48 hours, which eliminates internal stress while avoiding the appearance of large-particle MA structure that is not conducive to toughness.

[0020] Compared with the prior art, the advantages of the present invention are:

[0021] The present invention develops a composition system for obtaining ferrite + granular bainite structure under a slow cooling process, breaks through the upper limit of Mn content design, and provides a good composition design basis for obtaining ferrite + granular bainite structure under slow cooling rate by reasonably matching the contents of Cr, Ni, Mo and Cu on the basis of conventional Nb and Ti grain refinement. Secondly, a three-stage step slow cooling process is developed to accurately control the phase transformation process to obtain ferrite + granular bainite structure. On the basis of composition design, initial air cooling, step slow cooling and reasonable final cooling temperature control are used to provide conditions for the redistribution of carbon and alloy elements during the phase transformation process, and finally ferrite + granular bainite structure is obtained. Finally, an online stress relief treatment process is strictly designed, and the offline temperature and stack slow cooling time are strictly set through online cover stack slow cooling, which has the effect of eliminating internal stress and avoiding the generation of brittle structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a microstructure photograph of a 20 mm steel plate in an embodiment of the present invention. DETAILED DESCRIPTION

[0023] The present invention will be further described below with reference to examples.

[0024] Embodiment 1-2:

[0025] According to the chemical composition range and manufacturing method of the present invention, 500MPa low yield strength ratio bridge steel plate is manufactured through the process steps of converter smelting - LF refining - RH vacuum degassing - slab continuous casting - continuous casting slab inspection and cleaning - slab heating - high-pressure water descaling - controlled rolling - step cooling - cover pile slow cooling and the like.

[0026] This embodiment specifically lists two embodiments 1 and 2 with different process parameters. The specific processes of the heating, rolling and cooling stages of the two embodiments are as follows:

[0027] The continuous casting billet is heated to 1180-1200° C., the total heating time is 412 min (Example 1) / 425 min (Example 2), the soaking section holding time is 42 min (Example 1) and 45 min (Example 2), and the continuous casting billet is descaled with high-pressure water after being taken out of the furnace;

[0028] Then controlled rolling is performed, the starting rolling temperature in the rough rolling stage is 1050-1170°C (Examples 1 and 2), the reduction ratio in the rough rolling stage is 5.28 (Example 1) and 4.11 (Example 2), and the average reduction ratio in the last three passes is 27% (Example 1) and 22% (Example 2);

[0029] The finishing rolling temperature waiting thickness is 70 mm (Example 1) / 90 mm (Example 2), the finishing rolling start temperature is 830-850°C (Example 1) / 810-830°C (Example 2), the finishing rolling stage compression ratio is 3.5 (Example 1) and 3 (Example 2), and the final rolling temperature is 810-820°C (Example 1) and 800-810°C (Example 2);

[0030] After rolling, the steel sheet enters the cooling stage, which is first air-cooled, and the air-cooling termination temperatures are 745°C (Example 1) and 750°C (Example 2), respectively. Then, the steel sheet enters the water-cooling stage, and the cooling rate of the first stage of water-cooling is 5.2°C / s (Example 1) and 4.8°C / s (Example 2), and the temperature is 578°C (Example 1) and 584°C (Example 2); the cooling rate of the second stage of water-cooling is 7.6°C / s (Example 1) and 7.4°C / s (Example 2), and the final cooling temperature is 442°C (Example 1) and 456°C (Example 2).

[0031] After the steel plate is cooled, it is quickly taken off the line for slow cooling in a pile. The off-line temperatures are 360° C. (Example 1) and 378° C. (Example 2), respectively. A cover is added for slow cooling in the pile. The slow cooling time in the pile is ≥48 hours.

[0032] The chemical composition of the steel plates obtained in Examples 1 and 2 is shown in Table 1, the mechanical properties of the steel plates are shown in Table 2, and the microstructure of the steel plates is shown in Table Figure 1 shown.

[0033] Table 1 Chemical composition of the steel plate of the embodiment (wt.%)

[0034] Example C Si Mn Alt Nb Ti Cr Ni Cu Mo 1 0.06 0.31 1.65 0.03 0.048 0.015 0.15 0.15 0.15 0.12 2 0.07 0.28 1.72 0.03 0.052 0.014 0.16 0.21 0.22 0.21

[0035] Table 2 Mechanical properties of the steel plates in the examples

[0036] Yield strength ≥500MPa, tensile strength ≥700MPa, yield strength ratio ≤0.80, elongation ≥30%, impact energy at -40℃ ≥200J.

[0037]

[0038]

[0039] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for manufacturing a low yield strength ratio bridge steel plate, characterized in that The chemical composition of the steel plate includes, by mass percentage, C 0.04-0.07; Si 0.25-0.40; Mn 1.60-1.80; Alt 0.02-0.04; Nb 0.045-0.055; Ti 0.01-0.02; Cr 0.10-0.30; Ni 0.10-0.30; Cu 0.10-0.30; Mo 0.10-0.30; the balance is Fe and unavoidable impurities; the main steps of the method are: 1) The smelting raw materials are successively subjected to top and bottom blowing in a converter, LF+RH refining, and continuous casting to obtain a continuous casting billet of target thickness; 2) The continuous casting billet is heated in the furnace, the soaking section is kept at a temperature of 1180-1200°C, and the holding time is ≥40min; 3) A high compression ratio rolling process is adopted in the rolling stage, with a total compression ratio ≥10 and a final rolling temperature of 780-820°C; 4) After the steel plate is rolled, a step cooling process is designed, air cooling is performed after rolling, and then two-stage water cooling is performed. The cooling rate is accurately set by step to obtain a medium-temperature transformation structure of ferrite + granular bainite structure; 5) After the steel plate is cooled, it is quickly taken off the production line and covered with a pile for slow cooling. The off-line temperature is ≥350℃ and the slow cooling time is ≥48 hours; The stage cooling process is specifically as follows: air cooling within ≤30s after rolling, the air cooling final cooling temperature is 730-760°C, weak cooling within 30-50s, the cooling setting temperature is 560-600°C, the cooling rate range is set to 4-6°C / s, the cooling intensity is increased after >50s, the cooling rate range is set to 6-8°C / s, and the final cooling temperature is 400-450°C.

2. The method for manufacturing a low yield ratio bridge steel plate according to claim 1, characterized in that The steel plate has a yield strength of ≥500MPa, a tensile strength of ≥700MPa, a yield strength ratio of ≤0.80, an elongation of ≥30%, and an impact energy of ≥200J at -40°C.

3. The method for manufacturing a low yield ratio bridge steel plate according to claim 1, characterized in that The steel plate is produced by a controlled rolling and controlled cooling process to obtain a ferrite+granular bainite structure.

4. The method for manufacturing a low yield strength ratio bridge steel plate according to claim 1, characterized in that The compression ratio of the rough rolling stage of the rolling process is ≥4 times, the starting rolling temperature is 1050-1170°C, and the average reduction rate of the last three passes is ≥20%; the compression ratio of the finishing rolling stage is ≥3 times, and the starting rolling temperature is 800-860°C.