Polyamic acid, polyamic acid solution, polyimide, polyimide film, laminate, electronic device, and method for producing polyimide film

By using polyamic acid imide and nano-silica particles with a specific structure, the problem of improving Rth and colorability of polyimide substrates is solved, low thermal expansion and high transparency are achieved, and it is suitable for transparent displays and liquid crystals. monitor.

CN116348296BActive Publication Date: 2024-10-29KANEKA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180072116.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-18
Publication Date
2024-10-29
Estimated Expiration
2041-10-18

AI Technical Summary

Technical Problem

It is difficult in the existing technology to simultaneously reduce the linear expansion coefficient (Rth) and colorability of polyimide substrates while maintaining low thermal expansion, which affects its performance in transparent displays and liquid crystal displays.

Method used

Polyamic acid with a specific structure is used to form a polyimide film through its imide, and is treated at high temperatures to reduce Rth and colorability, combined with nano-silica particles to improve transparency and heat resistance.

Benefits of technology

It achieves low Rth, low coloration and low thermal expansion of the polyimide substrate, which is suitable for transparent displays and liquid crystal displays, and improves its stability and display performance in high-temperature processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116348296B_ABST
    Figure CN116348296B_ABST
Patent Text Reader

Abstract

The polyamic acid has a tetravalent organic group as a tetracarboxylic dianhydride residue, and has one or more selected from the group consisting of a p-phenylenediamine residue and a (2-phenyl-4-aminophenyl)-4-aminobenzoate residue as a diamine residue. The content of the tetravalent organic group as a tetracarboxylic dianhydride residue is 90 mol% or more and 100 mol% or less relative to all tetracarboxylic dianhydride residues. In the following general formula (1), R 1 and R 2 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, a hydroxyl group, a nitrile group, a nitro group, a carboxyl group, or an amide group. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polyamic acid, polyamic acid solution, polyimide, polyimide film, laminate, electronic device, and method for producing polyimide film. The present invention also relates to electronic device materials, thin film transistor (TFT) substrates, flexible display substrates, color filters, printed matter, optical materials, image display devices (more specifically, liquid crystal display devices, organic EL, electronic paper, etc.), 3D displays, solar cells, touch panels, transparent conductive film substrates, and alternative materials for components currently using glass using polyimide. Background Art

[0002] With the rapid development of electronic devices such as LCD, OLED, electronic paper, solar cells, touch panels, etc., the devices are becoming thinner, lighter, and more flexible. In these devices, polyimide is used as a substrate material instead of a glass substrate.

[0003] In these devices, various electronic components such as thin film transistors and transparent electrodes are formed on the substrate, and the formation of these electronic components requires high temperature processes. Polyimide has heat resistance sufficient to adapt to high temperature processes, and its linear expansion coefficient is close to that of glass substrates and electronic components, so it is not easy to generate internal stress and is suitable for substrate materials such as flexible displays.

[0004] Generally, aromatic polyimide is colored yellow-brown due to intramolecular conjugation and charge transfer (CT) complex formation, but in top-emitting organic EL, light is extracted from the opposite side of the substrate, so transparency is not required for the substrate, and conventional aromatic polyimide is used. However, in the case where light emitted from a display element is emitted through a substrate, such as in a transparent display, bottom-emitting organic EL, or liquid crystal display, or in the case where a sensor or camera component is arranged on the back of a substrate in order to make a full-screen display (without a notch) such as a smartphone, high optical properties (more specifically, low coloring, etc.) are also required for the substrate.

[0005] Furthermore, when a polyimide substrate is used for an image display device, if the retardation (Rth) in the thickness direction of the polyimide substrate is high, the display performance of the image display device tends to be reduced.

[0006] Under such circumstances, there is a demand for a material which has a linear expansion coefficient equivalent to that of conventional aromatic polyimide, has reduced coloration, and can achieve a low Rth.

[0007] As a plastic material with a small linear expansion coefficient (low thermal expansion) and high transparency, polyimide using a monomer with a rigid structure is known (for example, see Patent Document 1). In addition, Patent Document 2 states that a polyimide film with excellent transparency and heat resistance can be obtained by using a diamine having a fluorene structure.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2007-046054

[0011] Patent Document 2: Japanese Patent Application Publication No. 2016-179969 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] However, it is difficult to obtain a polyimide that can reduce Rth and has low coloring and low thermal expansion properties only by the techniques described in Patent Documents 1 and 2.

[0014] The present invention is made in view of the above situation, and its purpose is to provide a polyimide and a polyamic acid as a precursor thereof which can reduce Rth and have low coloring and low thermal expansion. Further, the purpose is to provide a product or component requiring low Rth, low coloring and low thermal expansion manufactured using the polyimide and the polyamic acid.

[0015] Solutions for solving problems

[0016] The polyamic acid of the present invention has a tetravalent organic group represented by the following general formula (1) as a tetracarboxylic dianhydride residue, and has one or more selected from the group consisting of a p-phenylenediamine residue and a (2-phenyl-4-aminophenyl)-4-aminobenzoate residue as a diamine residue. The content of the tetravalent organic group represented by the following general formula (1) is 90 mol% or more and 100 mol% or less relative to all tetracarboxylic dianhydride residues.

[0017]

[0018] In the above general formula (1), R 1 and R 2 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, a hydroxyl group, a nitrile group, a nitro group, a carboxyl group, or an amide group.

[0019] In one embodiment of the polyamic acid of the present invention, in the general formula (1), R 1and R 2 Both represent hydrogen atoms.

[0020] The polyamic acid according to one embodiment of the present invention further has, as a diamine residue, one or more selected from the group consisting of a 4,4′-diaminobenzanilide residue, a 2,2′-bis(trifluoromethyl)benzidine residue, and a 9,9-bis(4-aminophenyl)fluorene residue.

[0021] The polyamic acid solution of the present invention contains the polyamic acid of the present invention and an organic solvent.

[0022] The polyimide of the present invention is an imide of the polyamic acid of the present invention.

[0023] The glass transition temperature of the polyimide of the present invention is preferably 350° C. or higher.

[0024] The polyimide film of the present invention comprises the polyimide of the present invention.

[0025] The laminate of the present invention comprises a support and the polyimide film of the present invention.

[0026] The electronic device of the present invention comprises: the polyimide film of the present invention and an electronic element disposed on the polyimide film.

[0027] In the method for producing a polyimide film of the present invention, the polyamic acid solution of the present invention is applied onto a support to form a coating film containing the polyamic acid, and the coating film is heated to imidize the polyamic acid.

[0028] In one embodiment of the method for producing a polyimide film of the present invention, the maximum temperature when the coating film is heated is 380° C. or higher and 500° C. or lower.

[0029] In one embodiment of the method for producing a polyimide film of the present invention, the heating time at the maximum temperature is 5 minutes to 60 minutes.

[0030] In one embodiment of the method for producing a polyimide film of the present invention, the polyimide film obtained by heating the coating film is peeled from the support.

[0031] In one embodiment of the method for producing a polyimide film of the present invention, the polyimide film is peeled from the support by laser irradiation.

[0032] Effects of the Invention

[0033] The polyimide produced using the polyamic acid of the present invention can reduce Rth and has excellent low coloring and low thermal expansion. Therefore, the polyimide produced using the polyamic acid of the present invention is suitable as a material for electronic devices requiring low Rth, low coloring and low thermal expansion. DETAILED DESCRIPTION

[0034] Hereinafter, preferred embodiments of the present invention will be described in detail, but the present invention is not limited thereto.

[0035] First, the terms used in this specification are explained. "Structural unit" refers to a repeating unit constituting a polymer. "Polyamic acid" is a polymer containing a structural unit represented by the following general formula (2) (hereinafter sometimes referred to as "structural unit (2)").

[0036]

[0037] In the general formula (2), A 1 represents a tetracarboxylic dianhydride residue (a tetravalent organic group derived from tetracarboxylic dianhydride), A 2 It represents a diamine residue (a divalent organic group derived from a diamine).

[0038] The content of the structural unit (2) relative to all the structural units constituting the polyamic acid is, for example, 50 mol% to 100 mol%, preferably 60 mol% to 100 mol%, more preferably 70 mol% to 100 mol%, further preferably 80 mol% to 100 mol%, further more preferably 90 mol% to 100 mol%, and may be 100 mol%.

[0039] The "1% weight loss temperature" is a measurement temperature at which the weight of the polyimide at a measurement temperature of 150°C is reduced by 1% by weight relative to the weight of the reference (100% by weight).

[0040] Unless otherwise specified, the "linear expansion coefficient" refers to the linear expansion coefficient when the temperature drops from 350°C to 100°C (linear expansion coefficient when the temperature drops).

[0041] The "alkyl group having 1 to 12 carbon atoms" is linear or branched and unsubstituted. Examples of the alkyl group having 1 to 12 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, and n-dodecyl.

[0042] The "alkenyl group having 2 to 12 carbon atoms" is straight-chain or branched and unsubstituted. Examples of the alkenyl group having 2 to 12 carbon atoms include vinyl, 2-propenyl, 3-butenyl, 2-butenyl, 4-pentenyl, 3-pentenyl, 2-hexenyl, 3-hexenyl, 5-hexenyl, 2-heptenyl, 3-heptenyl, 4-heptenyl, 3-octenyl, 3-nonenyl, 4-decenyl, 3-undecenyl, and 4-dodecenyl.

[0043] The "alkoxy group having 1 to 12 carbon atoms" is straight-chain or branched and unsubstituted. Examples of the alkoxy group having 1 to 12 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, an n-pentoxy group, an isopentoxy group, a neopentoxy group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyloxy group, and an n-dodecyloxy group.

[0044] The "aryl group having 6 to 14 carbon atoms" is unsubstituted. Examples of the aryl group having 6 to 14 carbon atoms include an unsubstituted aromatic monocyclic hydrocarbon group having 6 to 14 carbon atoms, an unsubstituted aromatic condensed bicyclic hydrocarbon group having 6 to 14 carbon atoms, and an unsubstituted aromatic condensed tricyclic hydrocarbon group having 6 to 14 carbon atoms. More specific examples of the aryl group having 6 to 14 carbon atoms include phenyl, naphthyl, anthracenyl, and phenanthryl.

[0045] In the following, sometimes "system" is added after the compound name to collectively refer to the compound and its derivatives. When "system" is added after the compound name to indicate the name of a polymer, it means that the repeating unit of the polymer is derived from the compound or its derivative. In addition, tetracarboxylic dianhydride is sometimes recorded as "acid dianhydride".

[0046] The polyamic acid of the present embodiment has a tetravalent organic group represented by the following general formula (1) as a tetracarboxylic dianhydride residue, and has one or more selected from the group consisting of a p-phenylenediamine residue and a (2-phenyl-4-aminophenyl)-4-aminobenzoate residue as a diamine residue. The content of the tetravalent organic group represented by the following general formula (1) is preferably 90 mol% or more and 100 mol% or less relative to all tetracarboxylic dianhydride residues constituting the polyamic acid of the present embodiment.

[0047]

[0048] In the general formula (1), R 1 and R 2Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, a hydroxyl group, a nitrile group, a nitro group, a carboxyl group, or an amide group. 1 and R 2 , each independently preferably a hydrogen atom, a methyl group or an ethyl group, and particularly preferably R 1 and R 2 All represent hydrogen atoms. Therefore, as the tetravalent organic group represented by the general formula (1), a BPAF residue as a partial structure derived from 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (hereinafter sometimes referred to as "BPAF") is particularly preferred. That is, the polyamic acid of this embodiment particularly preferably has a BPAF residue as A in the general formula (2). 1 Unless otherwise specified, R in the general formula (1) is 1 and R 2 The description will be made by referring to the case of hydrogen atoms.

[0049] BPAF has a bulky fluorene structure, and thus can inhibit the formation of charge transfer (CT) complexes. Therefore, BPAF is suitable as a raw material (monomer) for polyimide with reduced coloration (low colorability). In addition, in polyimide using BPAF as a raw material (monomer), the fluorene ring derived from BPAF is twisted relative to the main chain, making it less likely to have birefringence. Therefore, BPAF is suitable as a raw material (monomer) for polyimide capable of reducing Rth.

[0050] When synthesizing the polyamic acid of the present embodiment, an acid dianhydride other than BPAF can be used as a monomer within a range that does not impair its performance. Examples of acid dianhydrides other than BPAF include pyromellitic dianhydride (hereinafter sometimes referred to as "PMDA"), 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter sometimes referred to as "BPDA"), p-phenylene bis(trimellitic anhydride), 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphenylene dicarboxylic dianhydride, and the like. Acid anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, dicyclohexyl-3,3',4,4'-tetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2'-oxodispiro[bicyclo[2.2.1]heptane-2,1'-cyclopentane-3',2"-bicyclo[2.2.1]heptane]-5,6:5",6"-tetracarboxylic dianhydride and derivatives thereof, which may be used alone or in combination of two or more.

[0051] In order to obtain a polyimide that can further reduce coloration and Rth, the content of BPAF residues relative to all tetracarboxylic dianhydride residues constituting the polyamic acid is preferably 92 mol% or more, more preferably 95 mol% or more, further preferably 97 mol% or more, and particularly preferably 100 mol% (having only BPAF residues as acid dianhydride residues).

[0052] When an acid dianhydride other than BPAF is used as a monomer, from the viewpoint of improving heat resistance and improving mechanical strength, the acid dianhydride other than BPAF is preferably selected from one or more of the group consisting of PMDA and BPDA, and more preferably PMDA. That is, when the polyamic acid of the present embodiment has an acid dianhydride residue other than BPAF residue as the acid dianhydride residue, the acid dianhydride residue other than BPAF residue is preferably selected from one or more of the group consisting of PMDA residue and BPDA residue, and more preferably PMDA residue.

[0053] When the polyamic acid of the present embodiment has one or more selected from the group consisting of PMDA residues and BPDA residues, from the viewpoint of reducing coloration and improving heat resistance and mechanical strength, the total content of PMDA residues and BPDA residues is preferably 1 mol % to 10 mol %, more preferably 3 mol % to 7 mol %, relative to all acid dianhydride residues constituting the polyamic acid.

[0054] When the polyamic acid of the present embodiment has one or more selected from the group consisting of PMDA residues and BPDA residues, from the viewpoint of reducing coloration and Rth and improving heat resistance and mechanical strength, the total content of BPAF residues, PMDA residues and BPDA residues relative to all acid dianhydride residues constituting the polyamic acid is preferably 91 mol % or more, more preferably 93 mol % or more, further preferably 95 mol % or more, still more preferably 97 mol % or more, and may also be 100 mol %.

[0055] In the polyamic acid of the present embodiment, as the diamine residue, there is one or more selected from the group consisting of a PDA residue as a partial structure derived from p-phenylenediamine (hereinafter sometimes described as "PDA") and a PHBAAB residue as a partial structure derived from (2-phenyl-4-aminophenyl)-4-aminobenzoate (hereinafter sometimes described as "PHBAAB"). That is, in the polyamic acid of the present embodiment, there is one or more selected from the group consisting of a PDA residue and a PHBAAB residue as A in the general formula (2). 2 Both PDA and PHBAAB have a rigid structure and are therefore suitable as a raw material (monomer) for polyimide having low thermal expansion.

[0056] The PDA residue is a divalent organic group represented by the following chemical formula (3). The PHBAAB residue is a divalent organic group represented by the following chemical formula (4).

[0057]

[0058] When synthesizing the polyamic acid of the present embodiment, diamines other than PDA and PHBAAB can be used as monomers within a range that does not impair its performance. Examples of diamines other than PDA and PHBAAB include 4,4'-diaminobenzanilide (hereinafter sometimes referred to as "DABA"), 2,2'-bis(trifluoromethyl)benzidine (hereinafter sometimes referred to as "TFMB"), 9,9-bis(4-aminophenyl)fluorene (hereinafter sometimes referred to as "BAFL"), 4-aminophenyl-4-aminobenzoate, 1,4-diaminocyclohexane, m-phenylenediamine, 4,4'-oxydiphenylamine, 3,4'-oxydiphenylamine, 2,2'-bis(trifluoromethyl)-4,4'- Diaminodiphenyl ether, N,N'-bis(4-aminophenyl)terephthalamide, 4,4'-diaminodiphenyl sulfone, m-tolidine, o-tolidine, 4,4'-bis(4-aminophenoxy)biphenyl, 2-(4-aminophenyl)-6-aminobenzoxazole, 3,5-diaminobenzoic acid, 4,4'-diamino-3,3'-dihydroxybiphenyl, 4,4'-methylenebis(cyclohexylamine), 1,3-bis(3-aminopropyl)tetramethyldisiloxane and derivatives thereof, which may be used alone or in combination of two or more.

[0059] In order to reduce the linear expansion coefficient, the total content of the PDA residue and the PHBAAB residue relative to all the diamine residues constituting the polyamic acid is preferably 0.1 mol% or more, and may be 1.0 mol% or more, 10.0 mol% or more, 30.0 mol% or more, 50.0 mol% or more, 70.0 mol% or more, 90.0 mol% or more, 99.0 mol% or more, or 99.9 mol% or more, or 100.0 mol%. In the polyamic acid of the present embodiment, as the diamine residue, only the PDA residue, only the PHBAAB residue, only the PDA residue and the PHBAAB residue, or at least one of the PDA residue and the PHBAAB residue and a diamine residue other than the PDA residue and the PHBAAB residue may be included.

[0060] When a diamine other than PDA and PHBAAB is used as a monomer, in order to further reduce coloration and Rth and further reduce the linear expansion coefficient, the diamine other than PDA and PHBAAB is preferably selected from the group consisting of DABA, TFMB and BAFL. That is, when the polyamic acid of the present embodiment has a diamine residue other than a PDA residue and a PHBAAB residue as a diamine residue, the diamine residue other than the PDA residue and the PHBAAB residue is preferably selected from the group consisting of DABA residue, TFMB residue and BAFL residue.

[0061] In order to further reduce the linear expansion coefficient, the polyamic acid of the present embodiment preferably has a DABA residue as a diamine residue. In the case where the polyamic acid of the present embodiment has a DABA residue, in order to further reduce the linear expansion coefficient, the content of the DABA residue is preferably 0.1 mol% or more relative to all the diamine residues constituting the polyamic acid, and can be 1.0 mol% or more, 10.0 mol% or more, 30.0 mol% or more, 50.0 mol% or more, 70.0 mol% or more, 90.0 mol% or more, or 99.0 mol% or more, and can also be 99.0 mol% or more and 99.9 mol% or less.

[0062] In order to further reduce coloration, the polyamic acid of the present embodiment preferably has a TFMB residue as a diamine residue. In the case where the polyamic acid of the present embodiment has a TFMB residue, in order to further reduce coloration, the content of the TFMB residue is preferably 0.1 mol% or more, and may be 1.0 mol% or more, 10.0 mol% or more, 30.0 mol% or more, 50.0 mol% or more, 70.0 mol% or more, 90.0 mol% or more, or 99.0 mol% or more and 99.9 mol% or less relative to all diamine residues constituting the polyamic acid.

[0063] In order to further reduce Rth, the polyamic acid of the present embodiment preferably has a BAFL residue as a diamine residue. In the case where the polyamic acid of the present embodiment has a BAFL residue, in order to further reduce Rth, the content of the BAFL residue is preferably 0.1 mol% or more, and can be 1.0 mol% or more, 10.0 mol% or more, or 30.0 mol% or more and 50.0 mol% or less relative to all diamine residues constituting the polyamic acid.

[0064] In the case where the polyamic acid of the present embodiment has one or more selected from the group consisting of a DABA residue, a TFMB residue, and a BAFL residue, in order to further reduce coloration and Rth and further reduce the linear expansion coefficient, the total content of the PDA residue, the PHBAAB residue, the DABA residue, the TFMB residue, and the BAFL residue relative to all the diamine residues constituting the polyamic acid is preferably 90.0 mol % or more, more preferably 93.0 mol % or more, further preferably 95.0 mol % or more, and even more preferably 97.0 mol % or more, and may also be 100.0 mol %.

[0065] In order to obtain a polyimide capable of further reducing coloration and Rth and further reducing the linear expansion coefficient, the polyamic acid of the present embodiment preferably satisfies the following condition 1, more preferably satisfies the following conditions 1 and 2, and further preferably satisfies the following conditions 1, 2, and 3. In particular, in order to reduce the linear expansion coefficient, it is preferred to satisfy the following conditions 1 and 4. In particular, in order to reduce coloration, it is preferred to satisfy the following conditions 1 and 5. In particular, in order to reduce Rth, it is preferred to satisfy the following conditions 1 and 6.

[0066] Condition 1: The polyamic acid has only a BPAF residue as an acid dianhydride residue.

[0067] Condition 2: The polyamic acid further has at least one selected from the group consisting of a DABA residue, a TFMB residue, and a BAFL residue as a diamine residue.

[0068] Condition 3: The total content of the PDA residue, the PHBAAB residue, the DABA residue, the TFMB residue, and the BAFL residue is 100.0 mol % with respect to all the diamine residues constituting the polyamic acid.

[0069] Condition 4: The polyamic acid has only a PDA residue and a DABA residue as diamine residues.

[0070] Condition 5: The polyamic acid has only a PDA residue and a TFMB residue, or only a PHBAAB residue and a TFMB residue as diamine residues.

[0071] Condition 6: The polyamic acid has only a PDA residue and a BAFL residue, or only a PDA residue and a PHBAAB residue as diamine residues.

[0072] From the viewpoint of suppressing the reduction of transparency caused by the residual unreacted monomers when the polyimide is formed, the molar ratio (molar ratio) obtained by dividing the total amount of tetracarboxylic dianhydride residues by the total amount of diamine residues is preferably 0.900 or more and less than 1.100, more preferably 0.950 or more and 1.080 or less. By adjusting the molar ratio within the above range, a polyimide with excellent transparency can be obtained.

[0073] The polyamic acid of the present invention can be synthesized by a known common method, for example, it can be obtained by reacting a diamine with a tetracarboxylic dianhydride in an organic solvent. The monomer components used in the synthesis of polyamic acid may also contain monomers other than diamine and tetracarboxylic dianhydride. For example, for the purpose of adjusting the molecular weight, a monofunctional amine or a monofunctional acid anhydride may also be used. An example of a specific synthesis method of polyamic acid is described. First, in an inert gas atmosphere such as argon or nitrogen, a diamine is dissolved in an organic solvent or dispersed in a slurry to prepare a diamine solution. Then, after the tetracarboxylic dianhydride is dissolved in an organic solvent or dispersed in a slurry, or in a solid state, it is added to the above-mentioned diamine solution.

[0074] When using diamine and tetracarboxylic dianhydride to synthesize polyamic acid, by adjusting the amount of diamine substance (the amount of each diamine substance when using multiple diamines) and the amount of tetracarboxylic dianhydride substance (the amount of each tetracarboxylic dianhydride substance when using multiple tetracarboxylic dianhydrides), the desired polyamic acid (polymer of diamine and tetracarboxylic dianhydride) can be obtained. The mole fraction of each residue in the polyamic acid is consistent with the mole fraction of each monomer (diamine and tetracarboxylic dianhydride) used in the synthesis of the polyamic acid. In addition, by mixing two kinds of polyamic acids, polyamic acid containing multiple tetracarboxylic dianhydride residues and multiple diamine residues can also be obtained. The temperature conditions of the reaction of diamine and tetracarboxylic dianhydride, i.e., the synthesis reaction of polyamic acid are not particularly limited, for example, in the range of 20°C or more and 150°C or less. The reaction time of the synthesis reaction of polyamic acid is, for example, in the range of 10 minutes or more and 30 hours or less.

[0075] The organic solvent used for the synthesis of the polyamic acid is preferably a solvent that can dissolve the tetracarboxylic dianhydride and diamine used, and more preferably a solvent that can dissolve the produced polyamic acid. As the organic solvent used in the synthesis of polyamic acid, for example, urea solvents such as tetramethylurea and N,N-dimethylethylurea; sulfoxide solvents such as dimethyl sulfoxide; sulfone solvents such as diphenyl sulfone and tetramethyl sulfone; amide solvents such as N,N-dimethylacetamide (DMAC), N,N-dimethylformamide (DMF), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), hexamethylphosphoric acid triamide; ester solvents such as γ-butyrolactone; halogenated alkyl solvents such as chloroform and dichloromethane; aromatic hydrocarbon solvents such as benzene and toluene; phenol solvents such as phenol and cresol; ketone solvents such as cyclopentanone; ether solvents such as tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, and p-cresol methyl ether. Usually these solvents can be used alone, or two or more can be used in combination as needed. In order to improve the solubility and reactivity of polyamic acid, the organic solvent used in the building-up reaction of polyamic acid is preferably selected from more than one solvent in the group consisting of amide solvents, ketone solvents, ester solvents and ether solvents, more preferably amide solvents (more specifically, DMF, DMAC, NMP etc.). In addition, the building-up reaction of polyamic acid is preferably carried out under inert gas atmospheres such as argon and nitrogen.

[0076] The weight average molecular weight of the polyamic acid of the present embodiment is also different according to its use, preferably 10,000 or more and 1,000,000 or less scope, more preferably 20,000 or more and 500,000 or less scope, more preferably 30,000 or more and 200,000 or less scope.When the weight average molecular weight is more than 10,000, it is easy to make a coating film or a polyimide film (film) with polyamic acid or the polyimide obtained using polyamic acid.On the other hand, when the weight average molecular weight is less than 1,000,000, sufficient solubility is shown for the solvent, so a coating film or a polyimide film with a smooth surface and uniform thickness can be obtained using the polyamic acid solution described later.The weight average molecular weight used herein refers to the polyethylene oxide conversion value measured using gel permeation chromatography (GPC).

[0077] The polyamic acid solution of the present embodiment comprises the polyamic acid and organic solvent of the present embodiment mentioned above.Herein, as the organic solvent contained in the polyamic acid solution, the organic solvent exemplified as the organic solvent that can be used in the synthesis reaction of polyamic acid can be cited, preferably selected from one or more solvents in the group consisting of amide solvents, ketone solvents, ester solvents and ether solvents, more preferably amide solvents (more specifically, DMF, DMAC, NMP, etc.).In the case of obtaining polyamic acid by the above-mentioned method, the reaction solution (reacted solution) itself can be used as the polyamic acid solution of the present embodiment.In addition, the solid polyamic acid obtained by removing the solvent from the reaction solution can be dissolved in an organic solvent, and the polyamic acid solution of the present embodiment is prepared.It should be noted that the content of the polyamic acid in the polyamic acid solution of the present embodiment is not particularly limited, for example, relative to the total amount of the polyamic acid solution, it is more than 1% by weight and less than 80% by weight.

[0078] The polyimide of the present embodiment is the imide of the polyamic acid of the present embodiment described above. The polyimide of the present embodiment can be obtained by a known method, and its manufacturing method is not particularly limited. Below, an example of a method for obtaining the polyimide of the present embodiment by imidizing the above-mentioned polyamic acid is described. Imidization is carried out by dehydrating and ring-closing the polyamic acid. The dehydration and ring-closing can be carried out by an azeotropic method, a thermal method or a chemical method using an azeotropic solvent. In addition, the imidization of polyamic acid to polyimide can adopt any ratio of more than 1% and less than 100%. That is, a part of the polyamic acid obtained by imidization can be synthesized. In particular, in the case of imidization by heating and temperature rise, the ring-closure reaction from polyamic acid to polyimide is carried out simultaneously with the hydrolysis of polyamic acid, and there is a possibility that the molecular weight when forming polyimide is lower than the molecular weight of polyamic acid, so it is preferred to imidize a part of the polyamic acid in the polyamic acid solution before forming the polyimide film described later from the viewpoint of improving mechanical properties. In this specification, a polyamic acid that has been partially imidized may also be described as a "polyamic acid".

[0079] The dehydration ring-closure of polyamic acid can be carried out as long as the polyamic acid is heated. The method for heating polyamic acid is not particularly limited. For example, after the polyamic acid solution of the present embodiment is coated on a support such as a glass substrate, a metal plate, a PET film (polyethylene terephthalate film), the heat treatment of polyamic acid is carried out in a range of more than 40 ° C and less than 500 ° C at a temperature. According to this method, a laminate of the present embodiment having a support and a polyimide film (in detail, a polyimide film of an imide compound of polyamic acid of the present embodiment) disposed on the support can be obtained. Alternatively, a polyamic acid solution is directly placed in a container subjected to a demoulding treatment such as a coating using a fluorine-based resin, and the polyamic acid solution is heated / dried under reduced pressure, thereby also being able to carry out the dehydration ring-closure of polyamic acid. By the dehydration ring-closure of polyamic acid based on these methods, polyimide can be obtained. It should be noted that the heating time of each of the above-mentioned processes is different according to the treatment capacity, the heating temperature of the polyamic acid solution for dehydration ring closure, and is usually preferably set to a range of more than 1 minute and less than 300 minutes, more than 5 minutes and less than 60 minutes after the treatment temperature reaches the maximum temperature. In addition, in order to shorten the heating time, show characteristics, imidizing agent and / or dehydration catalyst can be added to the polyamic acid solution, and the polyamic acid solution added with the imidizing agent and / or dehydration catalyst is heated by the above method to carry out imidization.

[0080] As the above-mentioned imidization agent, there is no particular limitation, and a tertiary amine can be used. As the tertiary amine, a heterocyclic tertiary amine is preferred. As preferred specific examples of the heterocyclic tertiary amine, pyridine, picoline, quinoline, isoquinoline, 1,2-dimethylimidazole, etc. can be cited. As the above-mentioned dehydration catalyst, acetic anhydride, propionic anhydride, n-butyric anhydride, benzoic anhydride, trifluoroacetic anhydride, etc. can be cited as preferred specific examples.

[0081] As the addition amount of imidizing agent, relative to the amide group of polyamic acid, preferably more than 0.5 times of molar equivalent and less than 5.0 times of molar equivalent, more preferably more than 0.7 times of molar equivalent and less than 2.5 times of molar equivalent, further preferably more than 0.8 times of molar equivalent and less than 2.0 times of molar equivalent. In addition, as the addition amount of dehydration catalyst, relative to the amide group of polyamic acid, preferably more than 0.5 times of molar equivalent and less than 10.0 times of molar equivalent, more preferably more than 0.7 times of molar equivalent and less than 5.0 times of molar equivalent, further preferably more than 0.8 times of molar equivalent and less than 3.0 times of molar equivalent. It should be noted that, in this specification, "amide group of polyamic acid" refers to the amide group generated by the polymerization reaction of diamine and tetracarboxylic dianhydride. When adding imidizing agent and / or dehydration catalyst in polyamic acid solution, it can be insoluble in organic solvent and directly added, or it can be added to be dissolved in organic solvent. In the method of adding directly without dissolving in an organic solvent, the imidization agent and / or dehydration catalyst may react rapidly and form a gel before diffusing. Therefore, it is preferred to add a solution obtained by dissolving the imidization agent and / or dehydration catalyst in an organic solvent to the polyamic acid solution.

[0082] The polyimide film of the present embodiment (specifically, the polyimide film containing the imide of the polyamic acid of the present embodiment) is colorless and transparent, has a low yellow index, and has a glass transition temperature (heat resistance) that can withstand the TFT manufacturing process, and is therefore suitable for a transparent substrate material for a flexible display. The content of the polyimide in the polyimide film of the present embodiment (specifically, the imide of the polyamic acid of the present embodiment) is, for example, 70% by weight or more relative to the total amount of the polyimide film, preferably 80% by weight or more, more preferably 90% by weight or more, and may also be 100% by weight. As components other than the polyimide in the polyimide film, for example, additives described later (more specifically, nano silica particles, etc.) may be cited.

[0083] The electronic device of this embodiment has: the polyimide film of this embodiment, and the electronic component directly or indirectly arranged on the polyimide film. When manufacturing the electronic device of this embodiment for use as a flexible display, first, an inorganic substrate such as glass is used as a support, and a polyimide film is formed thereon. Then, electronic components such as TFT are arranged (formed) on the polyimide film, thereby forming an electronic device on the support. The process of forming TFT is usually carried out in a wide temperature range of more than 150°C and less than 650°C, but in fact, in order to achieve the desired performance, an oxide semiconductor layer and an a-Si layer are sometimes formed at more than 300°C, and a-Si is crystallized using a laser or the like according to the situation.

[0084] At this time, if the thermal decomposition temperature of the polyimide film is low, outgas may be generated during the formation of electronic components, and it may adhere to the oven in the form of sublimates, causing contamination in the oven, or the inorganic film (barrier film described later) and the electronic component formed on the polyimide film may be peeled off, so the 1% weight loss temperature of the polyimide is preferably above 500°C. In more detail, before the formation of TFT, an inorganic film such as a silicon oxide film (SiOx film) and a silicon nitride film (SiNx film) is formed on the polyimide film as a barrier film. If the heat resistance of the polyimide is low, sometimes the polyimide and the inorganic film may be peeled off due to volatile components such as the decomposition gas of the polyimide in the high-temperature process after the inorganic film is stacked. Therefore, it is ideal that not only the 1% weight loss temperature of the polyimide is above 500°C, but also the weight loss rate when the polyimide is isothermally maintained at a temperature in the range of above 400°C and below 450°C is less than 1%.

[0085] In addition, when the glass transition temperature (Tg) of the polyimide is significantly lower than the process temperature, positional displacement may occur in the formation of electronic components, so the Tg of the polyimide is preferably 300°C or more, more preferably 350°C or more, and further preferably 400°C or more. The upper limit of the Tg of the polyimide is as high as possible, for example, 450°C. The Tg of the polyimide can be adjusted, for example, by changing the content of the residues with a rigid structure (more specifically, PDA residues, PHBAAB residues, etc.). In addition, the linear expansion coefficient of the glass substrate is usually smaller than that of the resin, so internal stress is generated between the glass substrate and the polyimide film. When the internal stress of the laminate of the glass substrate and the polyimide film used as a support is high, the laminate containing the polyimide film expands in the high-temperature TFT formation process, and shrinks when cooled to room temperature, causing problems such as warping, breakage of the glass substrate, and peeling of the polyimide film from the glass substrate. Therefore, the internal stress generated by the laminate of the polyimide film and the glass substrate is preferably less than 50MPa.

[0086] In order to suppress the generation of the above-mentioned internal stress, the linear expansion coefficient of the polyimide film is preferably 100ppm / K or less, more preferably 90ppm / K or less, and further preferably 80ppm / K or less. The linear expansion coefficient of the polyimide film may be -10ppm / K or more and 80ppm / K or less, 0ppm / K or more and 80ppm / K or less, 10ppm / K or more and 80ppm / K or less, 20ppm / K or more and 80ppm / K or less, 30ppm / K or more and 80ppm / K or less, 40ppm / K or more and 80ppm / K or less, or 50ppm / K or more and 80ppm / K or less.

[0087] In order to suppress the reduction in display performance when applied to an image display device, the thickness direction retardation (Rth) of the polyimide film for light of a wavelength of 550nm is preferably less than 200nm, more preferably less than 100nm, further preferably less than 90nm, further more preferably less than 80nm, and particularly preferably less than 70nm, calculated as a value of the polyimide film with a thickness of 10μm.

[0088] The transparency of the polyimide film can be evaluated by the total light transmittance (TT) based on JIS K7361-1:1997, the transmittance of light with a wavelength of 450nm (hereinafter sometimes referred to as "light transmittance"), and the haze based on JIS K7136-2000. When the polyimide film is used in an application requiring high transparency, the total light transmittance of the polyimide film is preferably 75% or more, more preferably 80% or more. In addition, when the polyimide film is used in an application requiring high transparency, the light transmittance of the polyimide film is preferably 75% or more, more preferably 78% or more. In addition, when the polyimide film is used in an application requiring high transparency, the haze of the polyimide film is preferably 1.5% or less, more preferably 1.2% or less, and further preferably less than 1.0%. In applications requiring high transparency, the polyimide film is required to have a high transmittance in the entire wavelength range, but the polyimide film has a tendency to easily absorb light on the short wavelength side, and the film itself is mostly colored yellow. In order to use the polyimide film in applications requiring high transparency, the yellowness index (YI) of the polyimide film is preferably 25 or less, more preferably 20 or less, further preferably 14 or less, and particularly preferably 12 or less. YI can be measured in accordance with JIS K7373-2006. The polyimide film imparted with transparency is suitable for transparent substrates for glass replacement purposes, etc., and substrates having sensors or camera modules disposed on the back.

[0089] In addition, there are two light extraction methods for flexible displays: a top emission method that extracts light from the surface side of the TFT and a bottom emission method that extracts light from the back side of the TFT. In the top emission method, since the light is not blocked by the TFT, it is easy to increase the aperture ratio and obtain high-definition image quality. The bottom emission method has the characteristics of easy alignment of the positions of the TFT and the pixel electrode and easy manufacturing. If the TFT is transparent, the aperture ratio can be increased even in the bottom emission method, so there is a tendency to adopt the bottom emission method that is easy to manufacture in large displays. The polyimide film of this embodiment has a low YI and excellent heat resistance, so it can also be applied to any of the above light extraction methods.

[0090] In the manufacturing process of electronic devices, electronic components such as thin film transistors and transparent electrodes are arranged on a substrate. The process for forming electronic components on a polyimide substrate is divided into a batch process and a roll-to-roll process. In the roll-to-roll process, electronic components are sequentially arranged on a polyimide substrate (polyimide film) while conveying a long strip of polyimide substrate. In the batch process, for example, a laminate is formed by arranging a polyimide substrate (polyimide film) on a glass support, and after the electronic components are arranged on the polyimide film of the laminate, the support is peeled off from the polyimide film. The polyimide of this embodiment can be applied to any process. The batch process is preferred in terms of cost because it can utilize the current equipment for glass supports.

[0091] The polyimide of the present embodiment can be suitably used as a material for display substrates such as TFT substrates and touch panel substrates. When polyimide is used for the above-mentioned purposes, the following method is mostly used: after an electronic device (in detail, an electronic device having an electronic component formed on a polyimide film) is formed on a support as described above, the polyimide film is peeled off from the support. In addition, as a material for the support, alkali-free glass is suitable for use. Below, an example of a method for manufacturing a polyimide film of the present embodiment and an example of a method for manufacturing a laminate (laminate of a polyimide film and a support) of the present embodiment are described in detail.

[0092] First, the polyamic acid solution of the present embodiment is applied on a support to form a laminate containing a coating film containing polyamic acid and a support containing a coating film. Then, the laminate containing the coating film is heated under conditions such as a temperature of more than 40°C and less than 200°C. The heating time at this time is, for example, more than 3 minutes and less than 120 minutes. It should be noted that a multi-stage heating process can also be provided, such as heating the laminate containing the coating film at a temperature of 50°C for 30 minutes and heating at a temperature of 100°C for 30 minutes. Then, in order to carry out the imidization of the polyamic acid in the coating film, the laminate containing the coating film (laminate containing a polyamic acid film) is heated under conditions such as a maximum temperature of more than 250°C and less than 500°C. The heating time at this time (heating time at the maximum temperature) is, for example, more than 1 minute and less than 300 minutes, preferably more than 5 minutes and less than 60 minutes. At this time, it is preferred to slowly heat up from a low temperature to the maximum temperature. The heating rate is preferably 2 ° C / minute or more and 10 ° C / minute or less, more preferably 4 ° C / minute or more and 10 ° C / minute or less. In addition, the maximum temperature is preferably in the range of 380 ° C or more and 500 ° C or less. When the maximum temperature is above 380 ° C, imidization is fully carried out, and when the maximum temperature is below 500 ° C, the thermal degradation of the polyimide can be suppressed. In addition, it is also possible to maintain any time at any temperature before reaching the maximum temperature. The imidization reaction can be carried out under air, under reduced pressure, or in an inert gas such as nitrogen. In order to show higher transparency, it is preferably carried out under reduced pressure or in an inert gas such as nitrogen. In addition, as a heating device, a known device such as a hot air oven, an infrared oven, a vacuum oven, an inert oven, a hot plate, etc. can be used. After these steps, the polyamic acid in the coating film is imidized, and a laminate (laminate of the present embodiment) of a support and a polyimide film (a polyimide film containing an imide of the polyamic acid of the present embodiment) can be obtained. In addition, by utilizing the method described later, the polyimide film formed on the support is peeled off from the support, so that the polyimide film of the present embodiment (the polyimide film comprising the imide of the polyamic acid of the present embodiment) can be obtained. Electronic components can be set on the polyimide film peeled off from the support. It should be noted that, in order to shorten the heating time and show characteristics, imidizing agent and dehydration catalyst can also be added to the polyamic acid solution, and the solution is heated and imidized by the above method.

[0093] The method of peeling the polyimide film from the obtained support and the laminate of the polyimide film can use a known method. For example, it can be peeled off by hand, or it can be peeled off using a mechanical device such as a driving roller or a robot. Furthermore, the following method can also be used: a method of providing a peeling layer between the support and the polyimide film; forming a silicon oxide film on a substrate having a plurality of grooves, forming a polyimide film using the silicon oxide film as a base layer, and infiltrating an etching solution of silicon oxide between the substrate and the silicon oxide film, thereby peeling off the polyimide film. In addition, a method of peeling off the polyimide film from the support by irradiation of a laser can also be used.

[0094] In addition, in the device manufacturing process of batch type, the adhesion between the preferred support and the polyimide film is excellent, and the device manufacturing process of the batch type refers to: polyamic acid solution is coated on a support such as a glass substrate, heated and imidized, and after forming electronic components, the polyimide film is peeled off. The adhesion mentioned here refers to the adhesion strength. After the polyimide film on the support forms electronic components, etc., the polyimide film formed with the electronic components, etc. is peeled off from the support. In such a manufacturing process, if the polyimide film and the support have excellent adhesion, it is possible to more accurately form or install electronic components, etc. In the manufacturing process of configuring electronic components, etc. across the polyimide film on the support, from the viewpoint of improving productivity, the peel strength between the support and the polyimide film is as high as possible. Specifically, the above-mentioned peel strength is preferably more than 0.05N / cm, more preferably more than 0.1N / cm.

[0095] In the manufacturing process as described above, when the polyimide film is peeled off from the laminate of the support and the polyimide film, the polyimide film is mostly peeled off from the support by laser irradiation. In this case, it is necessary to make the polyimide film absorb the laser, so the cut-off wavelength of the polyimide film is required to be longer than the wavelength of the laser used in the peeling. XeCl excimer laser with a wavelength of 308nm is mostly used in laser peeling, so the cut-off wavelength of the polyimide film is preferably above 312nm, more preferably above 330nm. On the other hand, if the cut-off wavelength is a long wavelength, there is a tendency for the polyimide film to be colored yellow, so the cut-off wavelength of the polyimide film is preferably below 390nm. From the viewpoint of both transparency (low yellow index) and processability of laser peeling, the cut-off wavelength of the polyimide film is preferably above 320nm and below 390nm, more preferably above 330nm and below 380nm. It should be noted that the cut-off wavelength in this specification refers to a wavelength with a transmittance of 0.1% or less measured by an ultraviolet-visible spectrophotometer.

[0096] The polyamic acid and polyimide of the present embodiment can be used directly in the coating and forming process for making products and components, and can also be used as a material for coating and other treatments of a film-shaped formed object. In order to be used in the coating or forming process, the polyamic acid or polyimide can be dissolved or dispersed in an organic solvent as required, and then, a photocurable component, a thermosetting component, a non-polymerizable binder resin and other components can be mixed as required to prepare a polyamic acid composition or a polyimide resin composition.

[0097] In order to give processing characteristics and various functionalities to the polyamic acid and polyimide of the present embodiment, various organic or inorganic low molecular weight compounds or high molecular weight compounds can be mixed in the polyamic acid solution as additives. As additives, for example, dyes, surfactants, leveling agents, plasticizers, silicones, microparticles, sensitizers, etc. can be used. Microparticles include: organic microparticles formed by polystyrene, polytetrafluoroethylene, etc.; inorganic microparticles formed by colloidal silica, carbon, layered silicates, etc., each of which can be a porous structure or a hollow structure. In addition, the function and form of the microparticles are not particularly limited, for example, they can be pigments, fillers, or fibrous particles.

[0098] In order to maintain the transparency of polyimide film and improve heat resistance, nano silica particles can be used as the above-mentioned additive, polyamic acid and nano silica particles are composited. From the viewpoint of maintaining the transparency of polyimide film, the average primary particle size of nano silica particles is preferably below 200nm, more preferably below 100nm, further preferably below 50nm, and can also be below 30nm. On the other hand, from the viewpoint of ensuring the dispersibility to polyamic acid, the average primary particle size of nano silica particles is preferably more than 5nm, more preferably more than 10nm. As the method for composite polyamic acid and nano silica particles, known methods can be used, for example, the method of using an organic silica sol dispersed with nano silica particles in an organic solvent can be enumerated. As a method for composite polyamic acid and nano-silica particles using organic silica sol, polyamic acid can be synthesized and then mixed with organic silica sol. In order to disperse the nano-silica particles more highly in the polyamic acid, it is preferred to synthesize the polyamic acid in the organic silica sol.

[0099] In addition, in order to improve the interaction with polyamic acid, the nano silicon dioxide particles can also be surface treated with a surface treatment agent. As a surface treatment agent, known surface treatment agents such as silane coupling agents can be used. As a silane coupling agent, it is widely known that there are alkoxysilane compounds with amino or glycidyl groups as functional groups, etc., which can be appropriately selected. In order to further improve the interaction with polyamic acid, as a silane coupling agent, an amino-containing alkoxysilane is preferably used. As an example of an amino-containing alkoxysilane, 3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 3-aminopropyl methyl dimethoxysilane, 3-aminopropyl methyl diethoxysilane, 3-(2-aminoethyl) aminopropyl trimethoxysilane, 3-phenylaminopropyl trimethoxysilane, 2-aminophenyl trimethoxysilane and 3-aminophenyl trimethoxysilane, etc., from the viewpoint of the stability of the raw material, preferably 3-aminopropyl triethoxysilane is used. As a surface treatment method for nano silica particles, a method of stirring a mixture of a silane coupling agent added to a dispersion (organic silica sol) at an atmospheric temperature of 20° C. or more and 80° C. or less can be cited. The stirring time at this time is, for example, 1 hour or more and 10 hours or less. At this time, a catalyst that promotes the reaction can be added.

[0100] The polyamic acid composition containing nano-silica particles formed by compositeization of polyamic acid and nano-silica particles preferably contains nano-silica particles in a range of more than 1 part by weight and less than 30 parts by weight relative to 100 parts by weight of polyamic acid, and more preferably contains nano-silica particles in a range of more than 1 part by weight and less than 20 parts by weight. When the content of nano-silica particles is more than 1 part by weight, the heat resistance of the polyimide containing nano-silica particles can be improved, and the internal stress can be fully reduced. When the content of nano-silica particles is less than 30 parts by weight, the mechanical properties and the adverse effects of the transparency of the polyimide containing nano-silica particles can be suppressed.

[0101] Imidazoles can also be added to the polyamic acid of the present embodiment as an additive for imparting the above-mentioned functionality. In this specification, imidazoles refer to compounds with 1,3-oxadiazole rings (1,3-oxadiazole ring structures). As imidazoles added in the polyamic acid of the present embodiment, there is no particular limitation, for example, 1H-imidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, etc. can be cited. Among these, preferably 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, more preferably 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole.

[0102] The content of imidazoles is preferably 0.005 mol or more and 0.1 mol or less relative to 1 mol of the amide group of polyamic acid, more preferably 0.01 mol or more and 0.08 mol or less, and further preferably 0.015 mol or more and 0.050 mol or less. By containing more than 0.005 mol of imidazoles, the film strength and transparency of the polyimide can be improved, and by making the content of imidazoles less than 0.1 mol, the storage stability of polyamic acid can be maintained and Tg and heat resistance can be improved.

[0103] The mixing method of polyamic acid and imidazoles is not particularly limited. From the viewpoint of the ease of molecular weight control of polyamic acid, it is preferred to add imidazoles in the polyamic acid after polymerization. At this time, imidazoles can be directly added to polyamic acid, or imidazoles can be dissolved in a solvent in advance, and the solution is added to polyamic acid, and the adding method is not particularly limited. Imidazoles can be added to the solution (reacted solution) of the polyamic acid after polymerization to prepare the polyamic acid solution (solution comprising polyamic acid and imidazoles) of the present embodiment.

[0104] In addition, in the polyamic acid solution of the present embodiment, in order to show the appropriate adhesion with the support, a silane coupling agent can be contained. The silane coupling agent can be added to the monomer solution before the polymerization reaction, can be added to the solution in the polymerization reaction, and can also be added to the polyamic acid solution after the polymerization reaction. For the type of the silane coupling agent, known substances can be used without particular restriction, and from the viewpoint of the reactivity with polyamic acid, particularly preferably the compound containing amino.

[0105] The blending ratio of the silane coupling agent to 100 parts by weight of the polyamic acid is preferably 0.01 parts by weight or more and 0.50 parts by weight or less, more preferably 0.01 parts by weight or more and 0.10 parts by weight or less, and further preferably 0.01 parts by weight or more and 0.05 parts by weight or less. By setting the blending ratio of the silane coupling agent to 0.01 parts by weight or more, the peeling-inhibiting effect on the support can be fully exerted, and by setting the blending ratio of the silane coupling agent to 0.50 parts by weight or less, the molecular weight reduction of the polyamic acid is suppressed, so that the embrittlement of the polyimide film can be suppressed.

[0106] Various inorganic thin films such as metal oxide thin films and transparent electrodes can be formed on the surface of the polyimide film of this embodiment. There is no particular limitation on the film-forming method of these inorganic thin films, and for example, PVD methods such as CVD, sputtering, vacuum evaporation, and ion plating can be cited.

[0107] The polyimide film of the present embodiment has heat resistance, low thermal expansion and transparency, and the internal stress generated when forming a laminate with a glass substrate is small, so it is preferably used in fields and products where these characteristics are effective. For example, the polyimide film of the present embodiment is preferably used in image display devices such as liquid crystal display devices, organic EL, electronic paper, printed matter, color filters, flexible displays, optical films, 3D displays, touch panels, transparent conductive film substrates, solar cells, etc., and more preferably as an alternative material for the part currently using glass. In these uses, the thickness of the polyimide film is, for example, more than 1 μm and less than 200 μm, preferably more than 5 μm and less than 100 μm. The thickness of the polyimide film can be measured using a laser holographic micrometer (Laser Hologage).

[0108] In addition, the polyamic acid solution of the present embodiment can be suitable for batch device manufacturing process, and the batch device manufacturing process refers to: coating polyamic acid solution on a support, heating and imidizing, forming electronic components, etc., and then peeling off the polyimide film. Therefore, in the present embodiment, a method for manufacturing electronic devices is also included, which includes coating polyamic acid solution on a support, heating and imidizing, and forming electronic components on the polyimide film formed on the support. In addition, the method for manufacturing electronic devices can also include the process of peeling off the polyimide film formed with electronic components, etc. from the support.

[0109] Example

[0110] Hereinafter, examples of the present invention will be described, but the scope of the present invention is not limited to the following examples.

[0111] <Measurement Methods of Physical Properties>

[0112] First, the method of measuring the physical properties of polyimide (polyimide film) will be described.

[0113] [Light transmittance]

[0114] The transmittance of each polyimide film obtained in the Examples and Comparative Examples described below at a wavelength of 450 nm was measured using an ultraviolet-visible-near-infrared spectrophotometer ("V-650" manufactured by JASCO Corporation).

[0115] [Yellow Index (YI)]

[0116] For each polyimide film obtained in the examples and comparative examples described below, the transmittance of light with a wavelength of 200 nm or more and 800 nm or less was measured using an ultraviolet-visible-near-infrared spectrophotometer ("V-650" manufactured by JASCO Corporation), and the yellow index (YI) of the polyimide film was calculated according to the formula described in JIS K7373-2006. When the YI is 14 or less, it is evaluated as "excellent in low coloring". On the other hand, when the YI exceeds 14, it is evaluated as "poor in low coloring".

[0117] [Haze]

[0118] The haze of each polyimide film obtained in the Examples and Comparative Examples described below was measured using an integrating sphere haze meter ("COH300A" manufactured by Nippon Denshoku Industries, Ltd.) according to the method described in JIS K7136-2000.

[0119] [Internal stress]

[0120] By the same method as in the examples and comparative examples described later, a polyimide film was formed on a glass substrate (material: alkali-free glass, thickness: 0.7 mm, size: 100 mm×100 mm) manufactured by Corning, the warpage of which was measured in advance, to obtain a laminate having a polyimide film with a thickness of 10 μm on the glass substrate. In order to eliminate the influence of water absorption of the polyimide film, the laminate was dried at 120° C. for 10 minutes, and then the warpage of the laminate in a nitrogen atmosphere at a temperature of 25° C. was measured using a thin film stress measuring device (“FLX-2320-S” manufactured by KLA-Tencor). Then, based on the warpage of the glass substrate before the polyimide film was formed and the warpage of the laminate, the internal stress generated between the glass substrate and the polyimide film was calculated by the Stoney formula.

[0121] [Delay]

[0122] For each polyimide film obtained in the examples and comparative examples described below, a phase difference meter ("OPTIPRO" manufactured by SINTEC) was used to measure the thickness direction retardation (Rth) for light with a wavelength of 550 nm. Then, based on the thickness D (unit: μm) of the measurement sample (polyimide film), the value (Rth) converted to a polyimide film with a thickness of 10 μm was calculated based on the following formula: 10 ). Rth 10 When the Rth is 80 nm or less, it is evaluated as "the delay can be reduced". 10 When the thickness exceeds 80 nm, it is evaluated as "the delay cannot be reduced".

[0123] R 10 =Rth×10 / D

[0124] [Coefficient of linear expansion (CTE)]

[0125] Each polyimide film obtained in the later-described embodiments and comparative examples was sampled with a width of 3 mm and a length of 10 mm and used as a sample for CTE measurement. Using a thermal analyzer ("TMA / SS7100" manufactured by Hitachi High-Tech Science Corporation), the sample was heated from 10°C to 400°C at a heating rate of 10°C / min under a load of 29.4 mN, and then cooled at a cooling rate of 40°C / min. Then, the CTE was calculated based on the strain from 350°C to 100°C during cooling. When CTE is less than 80ppm / K, it is evaluated as "excellent low thermal expansion". On the other hand, when CTE exceeds 80ppm / K, it is evaluated as "poor low thermal expansion".

[0126] [Glass transition temperature (Tg)]

[0127] Each polyimide film obtained in the following examples and comparative examples was sampled with a width of 3 mm and a length of 10 mm and used as a sample for Tg determination. A thermal analyzer ("TMA / SS7100" manufactured by Hitachi High-Tech Science Corporation) was used to apply a load of 98.0 mN to the sample, and the temperature was raised from 10°C to 450°C at 10°C / min, and the temperature and strain (elongation) were plotted to obtain a TMA curve. The temperature of the inflection point of the obtained TMA curve (the temperature corresponding to the peak in the differential curve of the TMA curve) was taken as the glass transition temperature (Tg).

[0128] [1% weight loss temperature (TD1)]

[0129] Each polyimide film obtained in the following examples and comparative examples (specifically, a polyimide film sampled in a manner to have a weight of 10 mg) was used as a sample for measurement. A differential thermal and thermogravimetric simultaneous measurement apparatus ("TG / DTA7200" manufactured by Hitachi High-Tech Science Corporation) was used. The temperature was raised from 25°C to 650°C at 20°C / min under a nitrogen atmosphere. The weight of the sample at a measurement temperature of 150°C was used as a reference, and the measurement temperature when the weight was reduced by 1% by weight relative to the reference was used as the 1% weight loss temperature (TD1).

[0130] <Production of Polyimide Film>

[0131] The following is a description of the method for preparing the polyimide film of the examples and comparative examples. It should be noted that the following abbreviations are used to describe the compounds and reagents. In addition, for the examples and comparative examples, the preparation of the polyamic acid solution was carried out under a nitrogen atmosphere.

[0132] NMP: N-methyl-2-pyrrolidone

[0133] BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride

[0134] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0135] PMDA: Pyromellitic Dianhydride

[0136] PDA: p-phenylenediamine

[0137] PHBAAB: (2-phenyl-4-aminophenyl)-4-aminobenzoate

[0138] TFMB: 2,2'-bis(trifluoromethyl)benzidine

[0139] DABA: 4,4'-diaminobenzanilide

[0140] BAFL: 9,9-bis(4-aminophenyl)fluorene

[0141] [Example 1]

[0142] First, a polyamic acid solution is prepared according to the following steps. In a 1L glass detachable flask equipped with a stirrer with a stainless steel stirring rod and a nitrogen inlet tube, 400.0g of NMP is placed as an organic solvent for polymerization. Then, 19.1g of PDA is placed in the flask while stirring the contents of the flask to dissolve it. Then, 80.9g of BPAF is added to the flask while stirring the contents of the flask, and then the contents of the flask are stirred for 24 hours at an atmosphere of 25°C. Then, NMP is added to the contents of the flask in such a way that the concentration of the polyamic acid in the contents of the flask after stirring becomes 10.0% by weight to obtain a polyamic acid solution.

[0143] Next, a spin coater is used to apply the obtained polyamic acid solution to a glass substrate ("EAGLE XG" manufactured by Corning, material: alkali-free glass, thickness: 0.7 mm, size: 150 mm × 150 mm), and heated at 80 ° C for 30 minutes in air to obtain a laminate having a film containing polyamic acid formed on a glass substrate (a laminate containing a polyamic acid film). Next, the laminate containing the polyamic acid film is heated under a nitrogen atmosphere under the following heating conditions to imidize the polyamic acid to obtain a laminate having a polyimide film having a thickness of 10 μm on a glass substrate. For the heating conditions during imidization, first, the atmosphere temperature is raised from 20 ° C to 350 ° C at a heating rate of 5 ° C / min, and maintained at 350 ° C for 30 minutes. Then, after the atmosphere temperature is raised to 420 ° C at a heating rate of 5 ° C / min, it is maintained at 420 ° C for 30 minutes. The polyimide film was peeled off from the glass substrate of the obtained laminated body, thereby obtaining the polyimide film of Example 1.

[0144] [Examples 2 to 35 and Comparative Examples 1 to 7]

[0145] The polyimide films of Examples 2 to 35 and Comparative Examples 1 to 7 were obtained by the same method as in Example 1, except that the types and ratios (charging ratios) of the acid dianhydride and the types and ratios (charging ratios) of the diamine were as shown in Tables 1 and 2. It should be noted that, for Examples 2 to 35 and Comparative Examples 1 to 7, the total amount of the acid dianhydride and the total amount of the diamine were the same as in Example 1.

[0146] For Examples 1 to 35 and Comparative Examples 1 to 7, the types and ratios of acid dianhydrides, and the types and ratios of diamines are shown in Tables 1 and 2. For Examples 1 to 35 and Comparative Examples 1 to 7, the molar fractions of the residues of polyamic acid in the prepared polyamic acid solutions are consistent with the molar fractions of the monomers (diamine and tetracarboxylic dianhydride) used in the synthesis of polyamic acid. It should be noted that in Examples 2 to 14 and 16 to 33, two kinds of diamines (component 1 and component 2) are used. In addition, in Example 34, Example 35 and Comparative Examples 4 to 7, two kinds of acid dianhydrides (component 1 and component 2) are used. For Examples 2 to 14, Examples 16 to 35 and Comparative Examples 4 to 7, component 1 and component 2 are placed in the flask at the same time. In addition, in Tables 1 and 2, the numerical values ​​of the ratios of acid dianhydrides are the content rates (unit: mole %) of each acid dianhydride relative to the total amount of acid dianhydrides used. In addition, in Table 1 and Table 2, the numerical value of the ratio of diamine is the content rate (unit: mol %) of each diamine with respect to the total amount of the diamine used.

[0147] [Table 1]

[0148]

[0149] [Table 2]

[0150]

[0151] <Measurement Results>

[0152] The measurement results of various physical properties of Examples 1 to 35 and Comparative Examples 1 to 7 are shown in Tables 3 and 4. In Tables 3 and 4, "-" means not measured. In Tables 3 and 4, "light transmittance" is the transmittance of light with a wavelength of 450 nm.

[0153] [Table 3]

[0154]

[0155] [Table 4]

[0156]

[0157] The polyamic acids synthesized in Examples 1 to 35 have BPAF residues as acid dianhydride residues. The polyamic acids synthesized in Examples 1 to 35 have one or more selected from the group consisting of PDA residues and PHBAAB residues as diamine residues. In the polyamic acids synthesized in Examples 1 to 35, the content of BPAF residues is 90 mol% or more and 100 mol% or less relative to all acid dianhydride residues.

[0158] In Examples 1 to 35, YI was 14 or less. Therefore, the polyimide films of Examples 1 to 35 were excellent in low coloration. 10 The polyimide films of Examples 1 to 35 were 80 nm or less. Therefore, the retardation was reduced in the polyimide films of Examples 1 to 35. In Examples 1 to 35, the CTE was 80 ppm / K or less. Therefore, the polyimide films of Examples 1 to 35 were excellent in low thermal expansion.

[0159] The polyamic acids synthesized in Comparative Examples 1 to 3 do not have one or more selected from the group consisting of PDA residues and PHBAAB residues as diamine residues. The polyamic acids synthesized in Comparative Examples 2 and 3 do not have BPAF residues as acid dianhydride residues. The polyamic acids synthesized in Comparative Examples 4 to 7 have a BPAF residue content of less than 90 mol% relative to all acid dianhydride residues.

[0160] In Comparative Example 1, CTE exceeded 80 ppm / K. Therefore, the polyimide film of Comparative Example 1 was not excellent in low thermal expansion. 10 It exceeded 80 nm. Therefore, the retardation could not be reduced in the polyimide film of Comparative Example 2. In Comparative Examples 2 to 7, the YI exceeded 14. Therefore, the polyimide films of Comparative Examples 2 to 7 were not excellent in low coloring property.

[0161] The above results show that the polyimide obtained from the polyamic acid of the present invention can reduce Rth and is excellent in low coloring property and low thermal expansion property.

Claims

1. A polyamic acid having only a tetravalent organic group represented by the following general formula (1) as a tetracarboxylic dianhydride residue, and having only a p-phenylenediamine residue and a 4,4′-diaminobenzanilide residue as diamine residues, In the general formula (1), R 1 and R 2 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryl group having 6 to 14 carbon atoms, a hydroxyl group, a nitrile group, a nitro group, a carboxyl group, or an amide group.

2. The polyamic acid according to claim 1, in, In the general formula (1), R 1 and R 2 Both represent hydrogen atoms.

3. The polyamic acid according to claim 1, in, The content of the 4,4′-diaminobenzanilide residue is 1.0 mol% or more relative to all diamine residues. A polyamic acid solution comprising the polyamic acid according to any one of claims 1 to 3 and an organic solvent. 5 . A polyimide which is an imide of the polyamic acid according to claim 1 . The polyimide according to claim 5 , which has a glass transition temperature of 350° C. or higher. 7 . A polyimide film comprising the polyimide according to claim 5 . 8 . A laminate comprising a support and the polyimide film according to claim 7 . 9 . An electronic device comprising: the polyimide film according to claim 7 , and an electronic element disposed on the polyimide film.

10. A method for producing a polyimide film, in, The polyamic acid solution according to claim 4 is applied onto a support to form a coating film containing the polyamic acid, and the coating film is heated to imidize the polyamic acid.

11. The method for producing a polyimide film according to claim 10, in, The maximum temperature when the coating film is heated is 380° C. or higher and 500° C. or lower.

12. The method for producing a polyimide film according to claim 11, in, The heating time at the maximum temperature is 5 minutes to 60 minutes.

13. The method for producing a polyimide film according to any one of claims 10 to 12, in, The polyimide film obtained by heating the coating film is peeled from the support.

14. The method for producing a polyimide film according to claim 13, in, The polyimide film is peeled off from the support by laser irradiation.

Citation Information

Patent Citations

  • Low tinted polyimide resin composition useful in optical application field, as well as method and composition relating to the same

    JP2007046054A

  • Diamine having fluorene skeleton, polyamic acid, and polyimide

    JP2016179969A

  • Optical film and image display device

    JP2005306983A

  • Polyimide precursor, resin composition containing the same, and cured product

    JP2020164597A