Catalyst for preparing anhydrous formaldehyde by dehydrogenation of methanol, preparation method and application thereof

By modifying the composite catalyst of phospho-aluminum molecular sieve and multi-metal oxide, the problem of low formaldehyde selectivity and yield in methanol dehydrogenation reaction is solved, and efficient and stable formaldehyde preparation is achieved, reducing production costs and energy consumption.

CN116351463BActive Publication Date: 2024-11-22PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111622408.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-11-22
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

The existing catalysts have low formaldehyde selectivity and yield in methanol dehydrogenation reaction, short service life of the catalyst, resulting in high production costs and unstable by-products at high temperatures, affecting process efficiency.

Method used

Using modified aluminum phosphate molecular sieve and multi-metal oxide composite catalysts, including nickel, copper, zinc and silver components, the acidity and structure of the catalyst are adjusted and catalyzed can be improved through the synergy between the modified aluminum phosphate molecular sieve and multi-metal oxide. Activity and stability.

Benefits of technology

It significantly improves methanol conversion and formaldehyde selectivity, extends the service life of the catalyst, reduces production costs, and achieves efficient dehydrogenation reaction at lower temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005092176600000021
    Figure GDA0005092176600000021
  • Figure GDA0005092176600000051
    Figure GDA0005092176600000051
  • Figure GDA0005092176600000061
    Figure GDA0005092176600000061
Patent Text Reader

Abstract

The present invention provides a catalyst for preparing anhydrous formaldehyde by dehydrogenating methanol, and a preparation method and application thereof, wherein the catalyst comprises a modified aluminum-phosphorus molecular sieve and a multinary metal oxide, wherein the modified aluminum-phosphorus molecular sieve is prepared by modifying an aluminum-phosphorus molecular sieve raw material with a modifier, wherein the modifier comprises an iron element and / or a titanium element, and the multinary metal oxide comprises a nickel component, a copper component, a zinc component and a silver component. The catalyst of the present invention has good catalytic activity and service life, and can efficiently catalyze the dehydrogenation reaction of methanol to prepare anhydrous formaldehyde, thereby improving the yield and selectivity of anhydrous formaldehyde.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic chemical catalysts, and in particular to a catalyst for preparing anhydrous formaldehyde by dehydrogenating methanol, and a preparation method and application thereof. Background Art

[0002] Formaldehyde is an important basic raw material for organic chemical industry, widely used in pesticides, medicines, dyes, and the production of thermosetting resins such as phenolic resins and melamine resins, and chemicals such as hexamethylenetetramine and pentaerythritol.

[0003] In recent years, the demand for anhydrous formaldehyde for engineering plastics and drugs such as urotropine with excellent synthetic properties has been increasing. At present, anhydrous formaldehyde is mainly obtained by removing water from industrial formaldehyde aqueous solution. Among them, the first method is to perform a distillation operation on commercial formaldehyde to separate formaldehyde from water. This process not only requires a large investment in equipment and operating costs, but also, given that the formaldehyde aqueous solution has a certain value of negative deviation relative to the ideal solution, resulting in the formation of an azeotropic system. Therefore, in the actual distillation operation, the dehydration separation effect is not good and the production cost is high; the first method is to heat and dissolve polyoxymethylene solid with methanol to obtain anhydrous formaldehyde, but polyoxymethylene itself is prepared by dehydration and condensation of 0.37-0.52 kg / L industrial formaldehyde aqueous solution, which is difficult to prepare and expensive, and has limited output. Therefore, this method has poor economic and practicality; the third method is to prepare anhydrous formaldehyde by extraction, that is, to obtain formaldehyde by extracting formaldehyde aqueous solution with alcohol compounds. This method requires adding an extraction section at the end of the process of the existing industrial device, which requires more equipment and operating costs. Developing a route to directly produce anhydrous formaldehyde from methanol and directly synthesizing anhydrous formaldehyde using catalytic dehydrogenation of methanol is considered to be an economical, environmentally friendly and green new process. This is mainly based on the following factors: First, this method does not produce water, which can save investment in distillation equipment and operating costs; second, this method can produce high-quality hydrogen as a by-product, and the product formaldehyde and by-product hydrogen are easy to separate, and there will be no problem of by-product formic acid corroding equipment in the methanol oxidation process.

[0004] According to relevant research, all possible reactions and their reaction heat in the direct dehydrogenation system of methanol are shown in Table 1. It can be seen from Table 1 that the methanol dehydrogenation reaction needs to absorb more heat than the formaldehyde decomposition reaction, and almost all other side reactions are exothermic reactions. Through the thermodynamic calculation of the methanol dehydrogenation reaction, it can be found that the methanol equilibrium conversion rate is 50% at 400°C, 90% at 500°C, and 99% at 700°C. Obviously, high temperature is conducive to the direct dehydrogenation reaction of methanol. However, under high temperature conditions, the thermodynamic trend of methanol completely dehydrogenating to CO is stronger than its partial dehydrogenation to HCHO, and the product is more stable. Further combined with the thermodynamic equilibrium composition of CH3OH, HCHO, CO, C, CH4 and H2, the study shows that the main products of methanol dehydrogenation at lower temperatures are methane and water, while carbon monoxide and hydrogen are preferably generated at high temperatures. Therefore, it is urgent to develop a catalyst suitable for methanol dehydrogenation to prepare anhydrous formaldehyde to promote the main reaction as much as possible and improve formaldehyde selectivity.

[0005] Table 1 Possible reactions and reaction heat in methanol dehydrogenation system

[0006]

[0007] Copper-based catalysts are catalysts commonly used in methanol dehydrogenation reactions. For example, patent document CN105732349 discloses a method for preparing anhydrous formaldehyde by dehydrogenating methanol. The dehydrogenation reaction of methanol is catalyzed by a copper-based catalyst. The copper-based catalyst is prepared by precipitating a soluble salt of copper and a soluble salt of a promoter on the surface of a molecular sieve carrier after dealuminization, and drying and calcining the soluble salt. The molecular sieve is one or more of ZSM-5, SAPO-11, SAPO-34, NaY, and HY, and the promoter is one or more of zinc, chromium, or potassium. There is also a multi-metal catalyst system. For example, patent document CN1546232A discloses an iron-molybdenum catalyst for preparing formaldehyde by oxidation of methanol and a preparation method thereof. The catalyst is a four-component catalyst system formed by adding chromium and vanadium oxides as promoters to an iron-molybdenum two-component catalyst system.

[0008] Although there have been studies and reports on catalysts for the dehydrogenation of methanol to produce anhydrous formaldehyde, the performance of the catalyst and the efficiency of formaldehyde production still need to be further improved, especially in terms of methanol conversion rate, formaldehyde yield and selectivity, and catalyst service life, which are still important issues faced by those skilled in the art. Summary of the invention

[0009] The present invention provides a catalyst for preparing anhydrous formaldehyde by dehydrogenating methanol, and a preparation method and application thereof. The catalyst has good catalytic activity and service life and other qualities, can efficiently catalyze the dehydrogenation reaction of methanol to prepare anhydrous formaldehyde, and improve the yield and selectivity of anhydrous formaldehyde.

[0010] In one aspect of the present invention, a catalyst for preparing anhydrous formaldehyde by dehydrogenation of methanol is provided, comprising a modified aluminum-phosphorus molecular sieve and a multinary metal oxide, wherein the modified aluminum-phosphorus molecular sieve is prepared by modifying an aluminum-phosphorus molecular sieve raw material with a modifier, wherein the modifier comprises iron and / or titanium, and the multinary metal oxide comprises a nickel component, a copper component, a zinc component and a silver component.

[0011] According to one embodiment of the present invention, the catalyst is in the shape of a toothed sphere, and its particle size is 2 mm to 3 mm.

[0012] According to one embodiment of the present invention, the mass ratio of the modifier to the phosphoaluminum molecular sieve raw material is (0.1-0.25):1; and / or, in the multinary metal oxide, the mass ratio of the nickel component, the copper component, the zinc component and the silver component, calculated as metal oxides, is (2-15):(2-5):(2-5):(1-5); and / or, the mass ratio of the modified phosphoaluminum molecular sieve and the multinary metal oxide is (20-40):(10-30).

[0013] According to one embodiment of the present invention, the aluminum-phosphorus molecular sieve raw material includes at least one of SAPO-5, SAPO-11, SAPO-31 and SAPO-34.

[0014] Another aspect of the present invention provides a method for preparing the above-mentioned catalyst, comprising: sequentially molding, drying and calcining a mixed system containing modified aluminum-phosphorus molecular sieve, a multi-metal compound, a peptizing agent, an extrusion aid, a binder and a solvent to obtain the catalyst; wherein the peptizing agent comprises an inorganic acid and / or an organic acid, and the multi-metal compound comprises a nickel compound, a copper compound, a zinc compound and a silver compound.

[0015] According to one embodiment of the present invention, the mixed system also includes a pH regulator, which includes at least one of hydrochloric acid solution, sulfuric acid solution, acetic acid solution, phosphoric acid solution, tartaric acid solution, ammonia water, and organic amine solution; based on the oxide of the metal in the multi-metal compound, based on the sum of the masses of the modified phosphoaluminum molecular sieve, the multi-metal compound, the peptizing agent, the extrusion aid, and the binder, the mass fraction of the multi-metal compound is 10% to 30%, the mass fraction of the modified phosphoaluminum molecular sieve is 20% to 40%, the mass fraction of the peptizing agent is 3% to 6%, the mass fraction of the extrusion aid is 2% to 10%, the mass fraction of the pH regulator is 0 to 5%, and the remainder is the binder.

[0016] According to one embodiment of the present invention, the nickel compound includes nickel oxide and / or nickel salt, the copper compound includes copper oxide and / or copper salt, the zinc compound includes zinc oxide and / or zinc salt, and the silver compound includes at least one of silver powder, silver oxide, and silver salt; and / or the peptizing agent includes at least one of nitric acid, hydrochloric acid, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, citric acid, salicylic acid, tartaric acid, and malic acid; and / or the extrusion aid includes at least one of sesbania powder, polyhydroxy acid, hydroxypropyl cellulose, graphite, and talc; and / or the binder includes pseudo-boehmite; and / or the solvent includes water.

[0017] According to one embodiment of the present invention, the drying temperature is 100° C. to 180° C., and the drying time is 3 h to 7 h; and / or the roasting temperature is 400° C. to 480° C., and the roasting time is 2 h to 6 h.

[0018] In another aspect of the present invention, a method for preparing anhydrous formaldehyde by dehydrogenating methanol is provided, comprising: subjecting a methanol-containing raw material to a dehydrogenation reaction under the action of the above-mentioned catalyst to obtain anhydrous formaldehyde.

[0019] According to one embodiment of the present invention, a mixed gas containing a methanol-containing raw material and a carrier gas is introduced into a reactor and contacts the catalyst in the reactor to carry out the dehydrogenation reaction. The reaction conditions are as follows: the reaction temperature is 400°C to 550°C, the reaction pressure is between normal pressure and 0.2 MPa, the mass content of the methanol-containing raw material in the mixed gas is 10% to 50%, and the mass space velocity of the methanol-containing raw material is 1 mL / g·s to 10.0 mL / g·s.

[0020] In the present invention, a modified aluminum-phosphorus molecular sieve modified by iron and / or titanium is used, and a multi-metal oxide is compounded at the same time, so that the catalytic activity, stability, service life and other qualities of the catalyst can be improved, and the methanol dehydrogenation reaction is efficiently catalyzed to prepare anhydrous formaldehyde, and the methanol conversion rate, as well as the selectivity and yield of formaldehyde are improved. Studies have shown that the methanol conversion rate can be as high as more than 78%, and the formaldehyde selectivity can be as high as more than 81%. In addition, the present invention also has the advantages of a simple catalyst preparation process and low cost, and a simple methanol dehydrogenation reaction process using the catalyst, low temperature, and low energy consumption, which is of great significance for actual industrial applications. DETAILED DESCRIPTION

[0021] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0022] The catalyst for preparing anhydrous formaldehyde by dehydrogenating methanol provided by the present invention comprises a modified aluminum-phosphorus molecular sieve and a multinary metal oxide. The modified aluminum-phosphorus molecular sieve is prepared by modifying an aluminum-phosphorus molecular sieve raw material with a modifier, the modifier comprises iron and / or titanium, and the multinary metal oxide comprises a nickel component, a copper component, a zinc component and a silver component.

[0023] The inventors have studied and analyzed that, under the catalyst composition system of the present invention, the synergistic effects between the components are as follows (I) to (III):

[0024] (I) Phosphorus aluminum molecular sieve has the characteristics of high specific surface area, rich pore structure and certain acidity. After modification with titanium and / or iron elements, the acidity of the modified phosphorus aluminum molecular sieve can be effectively regulated (the acidity data of the phosphorus aluminum molecular sieve raw material and the iron-modified phosphorus aluminum molecular sieve and titanium-modified molecular sieve measured at different temperatures are shown in Table 2), so that the acid-catalyzed methanol dehydrogenation reaction occurs during the methanol dehydrogenation reaction, avoiding the occurrence of side reactions such as the formation of dimethyl ether and water, and improving the selectivity and yield of formaldehyde;

[0025] Table 2 Acidity data of phosphorus aluminum molecular sieve and its modified

[0026]

[0027] Note: B(L) acid amount = A×S / m, A is absorbance, m is sample weight (g), S is the cross-sectional area of ​​the test sample (cm 2 ).

[0028] (II) Modified aluminum-phosphorus molecular sieves can also play the role of structural additives and modulating additives in catalysts. Specifically, modulating additives mainly change the chemical properties of the catalyst and the nature of the active center to achieve the purpose of changing the activation energy and improving the activity and selectivity of the catalyst. Modulating additives work by adjusting the electronic structure and geometric structure of the active components of the catalyst, including changing the electronegativity, work function, adsorption performance, electron migration performance, conductivity, acidity and alkalinity of the metal or metal ion of the catalyst, and the coordination environment of the central ion; structural additives mainly change the physical properties of the catalyst and change the number of active centers (without changing the activation energy). Structural additives can make the active components evenly dispersed and increase the surface area to improve the activity. They can also isolate microcrystals, prevent grain growth and sintering, and thus stabilize the structure. As a result, the catalyst of the present invention can exhibit good catalytic activity, selectivity, stability and other properties;

[0029] (III) The introduction of multi-metal oxides can avoid the problems of carbon deposition and deactivation of a single metal component and poor selectivity. For example, it can avoid the rapid decrease in catalyst activity and selectivity caused by the reduction of the metal components of the catalyst during the methanol dehydrogenation reaction, thereby ensuring the activity, stability and operating life of the catalyst. At the same time, through the synergistic effect of the multi-metal oxides and the modified aluminum phosphorus molecular sieve, the reduction rate of the multi-metal oxides can be reduced, and the ability of the catalyst acid center to receive electron pairs can be improved, thereby reducing the interaction between oxygen and hydrogen in the methanol hydroxyl group, effectively activating the hydroxyl group and improving the methanol conversion rate. At the same time, the introduction of the multi-metal oxides of the above-mentioned four components of nickel, copper, zinc and silver can adjust the electronic state with each other, change the d orbital electron density, and be more conducive to accepting electrons of the CH bond, thereby improving the methanol conversion rate and formaldehyde selectivity.

[0030] Specifically, aluminum phosphate molecular sieve (ALPO4-n), also known as aluminum phosphate molecular sieve or aluminum phosphate for short, is a type of porous material with aluminum phosphate as the framework and molecular sieve function. It was first synthesized in 1982 and is generally called the third generation molecular sieve. Its pore structure is uniform and regular, comparable to the molecular size, with a huge specific surface area, and the framework does not contain Si. The basic components are P, Al, and O. The basic units are [AlO4] and [PO4]. The two are strictly arranged alternately, making the framework as a whole electrically neutral. The orderly arrangement also makes the porous characteristics of the framework prominent, and has excellent thermal stability and hydrothermal stability. Table 3 shows some typical aluminum phosphate molecular sieves and their codes and framework characteristics.

[0031] Table 3 Some typical aluminum phosphorus molecular sieves and their codes and framework characteristics

[0032]

[0033] This type of molecular sieve framework is based on an equal amount of AlO4 - and PO4 + It is composed of tetrahedra, is electrically neutral, and exhibits weak acid properties. Taking AlPO4-5 molecular sieve as an example to further illustrate its structure, the AlPO4-5 molecular sieve skeleton topological structure belongs to the hexagonal crystal system, has a typical twelve-membered ring main channel, and the pore size is about 0.76nm.

[0034] According to the research of the present invention, the phosphorus aluminum molecular sieve raw material used generally preferably includes at least one of SAPO-5, SAPO-11, SAPO-31, and SAPO-34. After being modified by the above-mentioned modifier, the modified phosphorus aluminum molecular sieve formed is more conducive to compounding with the above-mentioned multi-metal oxides, thereby improving the catalytic activity and stability of the catalyst and other properties.

[0035] After further study, the mass ratio of the modifier to the phosphate aluminum molecular sieve raw material can be (0.1-0.25):1, for example, 0.1:1, 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.22:1, 0.25:1 or a range consisting of any two of them.

[0036] In the present invention, the phosphate aluminum molecular sieve raw material can be modified by conventional methods in the art to load iron and / or titanium to obtain a modified phosphate aluminum molecular sieve, for example, by an impregnation method (such as an equal volume impregnation method), which is not particularly limited.

[0037] Generally, in the multi-metal oxide, the nickel component exists in the form of nickel oxide (NiO), the copper component exists in the form of copper oxide (CuO), the zinc component exists in the form of zinc oxide (ZnO), and the silver component exists in the form of silver oxide (AgO). In some embodiments, the mass ratio of the nickel component, the copper component, the zinc component and the silver component is (2-15): (2-5): (2-5): (1-5) in terms of metal oxides. Specifically, the mass ratio of the nickel component (NiO), the copper component (CuO), the zinc component (ZnO) and the silver component (AgO) can be m Ni :m Cu :m Zn :m Ag , 2≤m Ni ≤15, 2≤m Cu ≤5, 2≤m Zn ≤5, 1≤m Ag ≤5, illustratively, m Ni is 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or a range consisting of any two of them, m Cu is 2, 2.5, 3, 3.5, 4, 4.5, 5 or any two thereof, m Zn is 2, 2.5, 3, 3.5, 4, 4.5, 5 or any two thereof, m Ag The range is 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 or any two thereof.

[0038] In some embodiments, the mass ratio of the modified aluminum-phosphorus molecular sieve and the multinary metal oxide is (20-40): (10-30), which can further optimize the catalyst performance and improve the selectivity of formaldehyde in the methanol dehydrogenation reaction product. Specifically, the mass ratio of the modified aluminum-phosphorus molecular sieve and the multinary metal oxide can be a:b, 20≤a≤40, 10≤b≤30, illustratively, a is 20, 22, 25, 28, 30, 32, 35, 38, 40 or any two thereof, and b is 10, 12, 15, 18, 20, 22, 25, 28, 30 or any two thereof.

[0039] In the present invention, the catalyst may be in the shape of a toothed ball, and its particle size is 2 mm to 3 mm, for example, 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm, 3 mm or any two thereof. The use of the toothed ball-shaped catalyst can reduce defects such as catalyst cost, bed pressure, and easy loss, further improve the catalytic activity of the catalyst, reduce the methanol dehydrogenation reaction temperature, and save energy consumption.

[0040] In one embodiment of the present invention, a method for preparing a catalyst is provided, comprising: sequentially molding, drying and calcining a mixed system containing a modified aluminum-phosphorus molecular sieve, a multi-metal compound, a peptizing agent, an extrusion aid, a binder and a solvent to obtain a catalyst.

[0041] Among them, the multi-metal compound includes nickel compound, copper compound, zinc compound and silver compound, the nickel compound includes nickel oxide and / or nickel salt, for example, including at least one of nickel nitrate, basic nickel carbonate, nickel oxide, nickel sulfate and nickel chloride, the copper compound includes copper oxide and / or copper salt, for example, including at least one of copper oxide, basic copper carbonate, copper nitrate and copper sulfate, the zinc compound includes zinc oxide and / or zinc salt, for example, including at least one of zinc oxide, zinc sulfate, zinc chloride, zinc nitrate and basic zinc carbonate, the silver compound includes at least one of silver powder, silver oxide and silver salt, for example, including at least one of silver powder, silver carbonate, silver chloride, silver sulfate, silver acetate, silver oxide and silver nitrate. Generally, after the above drying and roasting, the multi-metal compound forms multi-metal oxides such as NiO, CuO, ZnO and AgO.

[0042] In addition, the peptizing agent includes an inorganic acid and / or an organic acid, for example, at least one of nitric acid, hydrochloric acid, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, citric acid, salicylic acid, tartaric acid, and malic acid; the extrusion aid may include at least one of sesbania powder, polyhydroxy acid, hydroxypropyl cellulose, graphite, and talcum powder, and the polyhydroxy acid includes glycerol, etc., the binder may include pseudo-boehmite, and the solvent may specifically include water. The addition of peptizing agents, extrusion aids, binders, and other auxiliary agents can further regulate the acidity and pore structure of the catalyst and improve its catalytic activity, selectivity, stability, and other properties.

[0043] In addition, the above-mentioned mixed system may also include a pH regulator, which includes at least one of hydrochloric acid solution, sulfuric acid solution, acetic acid solution, phosphoric acid solution, tartaric acid solution, ammonia water, and organic amines. The organic amines include, for example, ethylenediamine and / or ethanolamine. In general, based on the sum of the masses of the modified aluminum-phosphorus molecular sieve, the aluminum-phosphorus compound, the peptizing agent, the extrusion aid, and the binder, the mass fraction of the multi-metal compound is 10% to 30%, for example, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, or a range consisting of any two thereof, and the mass fraction of the modified aluminum-phosphorus molecular sieve is 20% to 40%, for example, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 10 The mass fraction of the peptizing agent is 3-6%, for example, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% or a range consisting of any two of them, the mass fraction of the extrusion aid is 2-10%, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of them, the mass fraction of the pH adjusting agent is 0-5%, for example, 0, 1%, 2%, 3%, 4%, 5% or a range consisting of any two of them, and the balance is a binder.

[0044] In the above preparation process, the mixed system is shaped to initially form spherical particles, which are then dried and calcined to obtain the catalyst. In specific implementation, the particles can be dried to a water content (by mass) of less than 5% and then calcined. Generally, the drying temperature can be 100°C to 180°C, for example 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or a range consisting of any two thereof, the drying time is 3h to 7h, for example 3h, 4h, 5h, 6h, 7h or a range consisting of any two thereof, the calcination temperature is 400°C to 480°C, for example 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C or a range consisting of any two thereof, and the calcination time is 2h to 6h, for example 2h, 3h, 4h, 5h, 6h or a range consisting of any two thereof.

[0045] The method for preparing anhydrous formaldehyde by dehydrogenating methanol provided by the present invention comprises: subjecting raw materials containing methanol to a dehydrogenation reaction under the action of the above catalyst to obtain formaldehyde.

[0046] In a specific implementation, a mixed gas containing a methanol-containing raw material and a carrier gas can be introduced into a reactor, and contacted with the catalyst in the reactor to carry out the dehydrogenation reaction to obtain anhydrous formaldehyde. In some embodiments, the conditions for the dehydrogenation reaction are as follows: the reaction temperature is 400°C to 550°C, for example, 400°C, 420°C, 450°C, 480°C, 500°C, 520°C, 550°C or a range consisting of any two thereof; the reaction pressure is between normal pressure and 0.2 MPa; the mass content of the methanol-containing raw material in the mixed gas is 10% to 50%, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two thereof; the mass space velocity of the methanol-containing raw material is 1 mL / g·s to 10.0 mL / g·s, for example, 1 mL / g·s, 2 mL / g·s, 3 mL / g·s, 4 mL / g·s, 5 mL / g·s, 6 mL / g·s, 7 mL / g·s, 8 mL / g·s, 9 mL / g·s, 10 mL / g·s or a range consisting of any two thereof.

[0047] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Example 1

[0049] 20g of modified aluminum-phosphorus molecular sieve, multi-metal compound (10g in weight as metal oxide), 3g of peptizing agent (nitric acid + citric acid), 2g of extrusion aid, 2g of pH value regulator (concentrated ammonia water), 63g of pseudo-boehmite and deionized water were mixed to obtain a mixed system; the mixed system was sequentially molded, dried and calcined to prepare a toothed spherical catalyst CAT-01 with a particle size of 2.0mm;

[0050] Among them, the modified aluminum-phosphorus molecular sieve is an iron-modified SAPO-5 molecular sieve, and the mass ratio of iron to SAPO-5 molecular sieve is 0.1; the multi-metal compound consists of nickel nitrate, nickel oxide, copper sulfate, zinc nitrate, and silver powder, and the mass ratio of NiO, CuO, ZnO, and AgO is 5:2:2:1; the drying temperature is 100°C, and the drying time is 4h; the calcination temperature is 450°C, and the calcination time is 4h.

[0051] Referring to the process of Example 1, catalysts CAT-02 to CAT-08 of Examples 2 to 8, catalyst DCAT-01 of Comparative Example 1, and catalyst DCAT-02 of Comparative Example 2 were prepared respectively. In each example and comparative example, the composition of the modified aluminum-phosphorus molecular sieve is summarized in Table 4, the types of multi-metal compounds and their corresponding mass ratios of NiO, CuO, ZnO, and AgO are summarized in Table 5, the amount of modified aluminum-phosphorus molecular sieve, the amount of multi-metal compound (in terms of metal oxide), peptizing agent and its amount, extrusion aid and its amount, pH regulator and its amount, pseudo-boehmite amount, catalyst number, and catalyst particle size are summarized in Table 6.

[0052] Table 4 Composition of modified aluminum phosphorus molecular sieve in each embodiment

[0053]

[0054] Table 5 Multi-metal compounds in various examples

[0055]

[0056] Table 6 Amount of each material and catalyst particle size in each embodiment

[0057]

[0058] Note: When the auxiliary agent is composed of multiple substances, the mass of the auxiliary agent is the sum of the masses of the multiple substances. For example, in Example 1, the peptizing agent is composed of nitric acid and citric acid, and the sum of the masses of nitric acid and citric acid is 3g.

[0059] Application Examples

[0060] The process of preparing anhydrous formaldehyde by dehydrogenation of methanol is as follows: a mixed gas formed by methanol and a carrier gas enters a reactor, contacts with a catalyst in the reactor for a dehydrogenation reaction, and produces anhydrous formaldehyde; wherein the reaction pressure is 0.1 MPa, the mass content of the methanol raw material in the mixed gas is 30%, the mass space velocity of methanol is 6.0 mL / g·s, and the reaction temperature is shown in Table 7.

[0061] According to the above process, the above catalysts CAT-02 to CAT-08, DCAT-01, and DCAT-02 were used to carry out the process of preparing anhydrous formaldehyde by dehydrogenation of methanol, and the performance of each catalyst was evaluated. The measured methanol conversion rate and formaldehyde selectivity are shown in Table 7. Among them, the methanol conversion rate w = (x0-x1) / x0, x0 is the mass of the methanol raw material used before the reaction, and x1 is the residual mass of methanol after the reaction; the formaldehyde selectivity is determined according to the following process: the product after the dehydrogenation reaction is detected by high performance liquid chromatography (HPLC), and the total peak area of ​​the dehydrogenation reaction product is A 总 , where the peak area of ​​formaldehyde is A1, then formaldehyde selectivity = A1 / A 总 .

[0062] Table 7 Methanol dehydrogenation reaction temperature and reaction results using different catalysts

[0063]

[0064] The above describes the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A catalyst for preparing anhydrous formaldehyde by dehydrogenation of methanol, characterized in that: The invention comprises a modified aluminum-phosphorus molecular sieve and a multinary metal oxide, wherein the modified aluminum-phosphorus molecular sieve is prepared by modifying the aluminum-phosphorus molecular sieve raw material with a modifier, wherein the modifier comprises iron and / or titanium, and the multinary metal oxide comprises a nickel component, a copper component, a zinc component and a silver component; The mass ratio of the modifier to the phosphorus aluminum molecular sieve raw material is (0.1-0.25):1; The mass ratio of the modified aluminum-phosphorus molecular sieve to the multi-metal oxide is (20-35): (10-30); In the multi-metal oxide, calculated as metal oxide, the mass ratio of the nickel component to the copper component is (3-15):2, the mass ratio of the nickel component to the zinc component is (3-15):2, and the mass ratio of the nickel component to the silver component is (3-15):

1.

2. The catalyst according to claim 1, characterized in that The catalyst is in the shape of a toothed sphere, and its particle size is 2 mm to 3 mm.

3. The catalyst according to claim 1, characterized in that The phosphorus aluminum molecular sieve raw material includes at least one of SAPO-5, SAPO-11, SAPO-31, and SAPO-34.

4. A method for preparing the catalyst according to any one of claims 1 to 3, characterized in that: include: The catalyst is prepared by molding, drying and calcining a mixed system containing the modified aluminum-phosphorus molecular sieve, a multi-metal compound, a peptizing agent, an extrusion aid, a binder and a solvent in sequence; wherein the peptizing agent includes an inorganic acid and / or an organic acid, and the multi-metal compound includes a nickel compound, a copper compound, a zinc compound and a silver compound.

5. The method for preparing the catalyst according to claim 4, characterized in that: The mixed system further includes a pH adjuster, and the pH adjuster includes at least one of hydrochloric acid solution, sulfuric acid solution, acetic acid solution, phosphoric acid solution, tartaric acid solution, ammonia water, and organic amine solution; Calculated as the oxide of the metal in the multinary metal compound, based on the sum of the masses of the modified phosphoaluminum molecular sieve, the multinary metal compound, the peptizing agent, the extrusion aid and the binder, the mass fraction of the multinary metal compound is 10% to 30%, the mass fraction of the modified phosphoaluminum molecular sieve is 20% to 40%, the mass fraction of the peptizing agent is 3% to 6%, the mass fraction of the extrusion aid is 2% to 10%, the mass fraction of the pH adjuster is 0 to 5%, and the remainder is the binder.

6. The method for preparing the catalyst according to claim 4, characterized in that: The nickel compound includes nickel oxide and / or nickel salt, the copper compound includes copper oxide and / or copper salt, the zinc compound includes zinc oxide and / or zinc salt, and the silver compound includes at least one of silver powder, silver oxide and silver salt; and / or, The peptizing agent comprises at least one of nitric acid, hydrochloric acid, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, citric acid, salicylic acid, tartaric acid and malic acid; and / or, The extrusion aid comprises at least one of sesbania powder, polyhydroxy acid, hydroxypropyl cellulose, graphite and talc; and / or, The binder comprises pseudo-boehmite; and / or, The solvent includes water.

7. The method for preparing a catalyst according to claim 4, characterized in that: The drying temperature is 100° C. to 180° C., and the drying time is 3 h to 7 h; and / or, The calcination temperature is 400° C. to 480° C., and the calcination time is 2 h to 6 h.

8. A method for preparing anhydrous formaldehyde by dehydrogenation of methanol, characterized in that: include: A methanol-containing raw material is subjected to a dehydrogenation reaction under the action of a catalyst according to any one of claims 1 to 3 or a catalyst prepared by the method for preparing a catalyst according to any one of claims 4 to 7 to prepare anhydrous formaldehyde.

9. The method for preparing anhydrous formaldehyde by dehydrogenation of methanol according to claim 8, characterized in that: A mixed gas containing a methanol-containing raw material and a carrier gas is allowed to enter a reactor and contact the catalyst in the reactor to carry out the dehydrogenation reaction. The reaction conditions are as follows: a reaction temperature of 400° C. to 550° C., a reaction pressure between normal pressure and 0.2 MPa, a mass content of the methanol-containing raw material in the mixed gas of 10% to 50%, and a mass space velocity of the methanol-containing raw material of 1 mL / g·s to 10.0 mL / g·s.