Preparation method and application of a multifunctional color-developing double metal hydroxide

By preparing color-developing bimetallic hydroxides in concrete, using their layered structure to capture sulfate ions and distinguish distribution through color-developing, the crack erosion problem of concrete in marine environment is solved, and the durability and use of concrete are significantly improved. life.

CN116354638BActive Publication Date: 2024-11-22JIANGSU UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310191290.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-02
Publication Date
2024-11-22
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

Concrete is susceptible to erosion of sulfate ions in marine environments, causing crack expansion and protective layer to fall off, and existing bimetallic hydroxides are difficult to intuitively distinguish their distribution range.

Method used

Sodium metaaluminate powder and ferrous lactate powder or calcium nitrite powder are combined to simulate the reaction of pore solutions in seawater and concrete to prepare color-developed bimetallic hydroxides, and sulfate ions are captured using layered structures and pass through brown-red Distribution range is distinguished from white marks.

Benefits of technology

Effectively fill cracks, prevent erosion ions from entering, improve concrete durability, and intuitively analyze the distribution range through color rendering to extend the service life of offshore construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116354638B_ABST
    Figure CN116354638B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a multifunctional color-developing double metal hydroxide, the preparation method comprising the following steps: uniformly mixing a simulated seawater solution with a simulated pore solution of concrete, adding a combination of ferrous lactate powder, sodium metaaluminate powder, and calcium nitrite powder of a target design, obtaining a solid mixture and a clear liquid after standing, and filtering to obtain a solid substance. The present invention is to prepare a brown-red and white distinguishable double metal hydroxide by ferrous lactate powder, sodium metaaluminate powder, and calcium nitrite powder, such double metal hydroxide can not only effectively block cracks, but also can distinguish the type and distribution of double metal hydroxides in the crack area by color, in addition, it can also efficiently fix corrosive sulfate ions, and has a wide range of application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a metal hydroxide, and in particular to a preparation method and application of a multifunctional color-developing double metal hydroxide. Background Art

[0002] Concrete is the most widely used and consumed building material in modern civil engineering. Because its raw materials are very abundant, extremely common in nature, can be obtained locally, and are inexpensive, concrete has a certain resistance to changes such as heat and cold, freeze-thaw, dry and wet, wind and rain erosion, external force impact, water scouring, and practical wear. Under normal use, it is an engineering material with a relatively long life. It has been widely used in marine projects such as ports, docks, cross-sea bridges and undersea tunnels. In the future development of marine architecture, concrete will still be the most important and indispensable construction material in civil engineering.

[0003] The ocean is a harsh service environment for concrete. In the marine environment, when cracks occur in concrete, a large number of sulfate ions will penetrate into the concrete through the crack channels, causing the concrete volume to expand and the concrete protective layer to crack or even fall off, seriously endangering the practicality and safety of the concrete structure. Common double metal hydroxides are white, the same color as the surface calcium carbonate and calcium hydroxide, and it is difficult to intuitively distinguish the product type and distribution range. Therefore, it is urgent to find a metal hydroxide that can both inhibit corrosive ions and develop color. Summary of the invention

[0004] Purpose of the invention: The present invention aims to provide a method for preparing a multifunctional color-developing double metal hydroxide that can effectively fill crack areas. The method can intuitively reflect the distribution of the product through color, avoiding the use of complex means to detect the product; another purpose of the present invention is to provide a multifunctional color-developing double metal hydroxide obtained by the preparation method for use in crack repair and fixation of corrosive ions in marine engineering structures.

[0005] Technical solution: The preparation method of the multifunctional color-developing double metal hydroxide of the present invention comprises the following steps:

[0006] (1) preparing a simulated seawater solution, adding the simulated concrete pore solution thereto, and mixing them evenly;

[0007] (2) adding a combination of sodium aluminate powder and ferrous lactate powder, or a combination of ferrous lactate powder, sodium aluminate powder and calcium nitrite powder to the mixed solution to react and obtain a mixed solution;

[0008] (3) filtering the mixture solution to obtain a mixture solid, and drying the solid to obtain the multifunctional color-developing double metal hydroxide.

[0009] Furthermore, in step (1), an equal volume of a reagent for simulating pore solution of concrete is added to the simulated seawater.

[0010] Furthermore, in the simulated seawater solution in step (1), the chloride ion concentration is 0.490-0.500 mol / L, and the sulfate ion concentration is 0.025-0.035 mol / L.

[0011] Furthermore, in step (2), the mass ratio of the ferrous lactate powder to the sodium aluminate powder is 1:0.3-0.4; the mass ratio of the sodium aluminate powder, the ferrous lactate powder and the calcium nitrite powder is 0.3-0.4:1:0.7-0.8.

[0012] Furthermore, the solution reaction time in step (2) is 14 to 28 days.

[0013] Furthermore, the drying temperature in step (3) is 40-50°C and the drying time is more than 12 hours.

[0014] Furthermore, the double metal hydroxide obtained after drying is brown-red or a mixture of white and brown-red.

[0015] The multifunctional color-developing double metal hydroxide prepared by the preparation method can be applied in marine engineering buildings.

[0016] The multifunctional color-developing double metal hydroxide is used for crack repairing, and different types of double metal hydroxides are marked by brown-red or a mixture of brown-red and white to distinguish the distribution range of the double metal hydroxides; the double metal hydroxide also has a highly efficient fixing effect on corrosive sulfate ions.

[0017] To test the fixation of the brown-red double metal hydroxide on sulfate ions, the dosage ratio of ferrous lactate and sodium aluminate powder was adjusted to 1:1.2, 1:1.4, 1:1.6, 1:1.8, and 1:2.0. The sulfate ion concentration is difficult to measure directly. The test method is as follows: ① Mix 1ml of 1mol / L barium chloride solution, 6ml of deionized water, and 1ml of hydrochloric acid with 2ml of the solution to be tested; ② Test the OD of the mixed solution. 405 The sulfate ion concentration is then calculated using the fitting formula. The fitting formula is as follows.

[0018]

[0019] Where:

[0020] ρ——sulfate ion concentration, mol / L;

[0021] OD 405——The coagulation solution absorbs light at a wavelength of 405nm.

[0022] Principle of the invention: The double metal hydroxide obtained by the preparation method of the present invention is a layered double metal hydroxide, which is a special layered material composed of positively charged layers and interlayer balanced anions; the layers are composed of divalent and trivalent metal hydroxides, and the anions of the interlayers are used to make up for the charge balance of the layers, so that the layered double metal hydroxide exhibits electrical neutrality as a whole. The interlayer anions of the layered double metal hydroxide are exchangeable and are replaced by other anions during the preparation process. In the process of self-repair, the anions contained in the interlayers of the double metal hydroxide are released by the stimulation of external corrosive media, while capturing SO4 2- Corrosive anionic substances.

[0023] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The double metal hydroxide can effectively fill the crack area and prevent the corrosive ions from rushing into the concrete to accelerate the destruction; (2) The double metal hydroxide marks different types of double metal hydroxides by brown-red and white colors to distinguish the distribution range of double metal hydroxides, which provides an intuitive analysis of the distribution range of the action range of bimetallic minerals; (3) The double metal hydroxide prepared by the preparation method has an efficient fixation effect on sulfate corrosive ions in seawater, improves the durability of concrete, and ensures the service life of marine engineering structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is an image of a white double hydroxide;

[0025] Figure 2 It is an image of a maroon double hydroxide;

[0026] Figure 3 The color difference of mixed group double metal hydroxides;

[0027] Figure 4 The microscopic morphology is white product and brown-red product;

[0028] Figure 5 This is a test result diagram of the fixation effect of brown-red double metal hydroxide on sulfate ions;

[0029] Figure 6 This is a test result of the fixation effect of brown-red and white mixed double metal hydroxide on sulfate ions. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0031] Example 1

[0032] (1) Prepare 150 ml of simulated seawater solution according to Table 1, add an equal volume of the agent for simulating concrete pore solution prepared according to Table 2, stir evenly and set aside for use. The chloride ion concentration in the simulated solution is measured to be 0.494 mol / L, and the sulfate ion concentration is 0.029 mol / L;

[0033] (2) Weigh 13.325 g of ferrous lactate powder and 4.725 g of sodium aluminate powder, respectively, and add them to the above solution;

[0034] (3) After the solution reacted for 28 days, sediment was found at the bottom of the three solutions. The three solutions were filtered to obtain sediment and clear solution. The sediment was dried at 40 °C for 12 h to obtain a brown-red product ( Figure 2 ); add deionized water to the filtered clear solution to restore its volume to 150 ml.

[0035] Example 2

[0036] (1) Prepare 150 ml of simulated seawater solution according to Table 1, add an equal volume of the agent for simulating concrete pore solution prepared according to Table 2, stir evenly and set aside for use. The chloride ion concentration in the simulated solution is measured to be 0.494 mol / L, and the sulfate ion concentration is 0.029 mol / L;

[0037] (2) Weigh 4.725 g, 13.325 g, and 9.451 g of sodium aluminate powder, ferrous lactate powder, and calcium nitrite powder, respectively, and add them to the above solution;

[0038] (3) After the solution reacted for 28 days, sediment was found at the bottom of the solution. The solution was filtered to obtain sediment and clear liquid. The sediment was dried at 40 °C for 12 h to obtain a white and brown-red mixed product ( Figure 3 ); add deionized water to the filtered clear solution to restore its volume to 150 ml.

[0039] Comparative Example

[0040] (1) Prepare 150 ml of simulated seawater solution according to Table 1, add an equal volume of the agent for simulating concrete pore solution prepared according to Table 2, stir evenly and set aside for use. The chloride ion concentration in the simulated solution is measured to be 0.494 mol / L, and the sulfate ion concentration is 0.029 mol / L;

[0041] (2) Weigh 7.522 g of calcium nitrite powder and 4.725 g of sodium aluminate powder.

[0042] (3) After the solution reacted for 28 days, sediment was found at the bottom of the three solutions. The three solutions were filtered to obtain sediment and clear solution. The sediment was dried at 40°C for 12 hours to obtain a white product ( Figure 1 ); add deionized water to the filtered clear solution to restore its volume to 150 ml.

[0043] The microscopic morphologies of the white and brown-red products of Comparative Example 1 and Example 1 are as follows: Figure 4 As shown, its microstructure presents a lamellar structure, and its structure is that the interlayer plates carry anions, and the anions carried by the interlayer plates are exchangeable, and this property is used to adsorb a large amount of corrosive ions.

[0044] The total amount of the combined powder of ferrous lactate and sodium aluminate was adjusted so that the total mass of the combined powder of Example 1 and its mass ratio were 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2.0 (the mass ratio of ferrous lactate to sodium aluminate remained unchanged), and the fixation effect of Example 1 and the brown-red double metal hydroxide obtained by adding the above-mentioned combined powder on sulfate ions was tested. The test results are as follows: Figure 5 As shown; the total amount of the combined powder of sodium aluminate powder, ferrous lactate powder and calcium nitrite powder was adjusted so that the total mass of the combined powder of Example 2 and its mass ratio were 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2.0 (the mass ratio of sodium aluminate powder, ferrous lactate powder and calcium nitrite powder remained unchanged), and the fixation effect of Example 2 and the brown-red and white mixed double metal hydroxide obtained by adding the above-mentioned combined powder on sulfate ions was tested. The test results are as follows Figure 6 The sulfate ion concentration is difficult to measure directly. The test method is as follows: ① Mix 1 ml of 1 mol / L barium chloride solution, 6 ml of deionized water, and 1 ml of hydrochloric acid with 2 ml of the solution to be tested; ② Test the OD of the mixed solution. 405 The sulfate ion concentration is then calculated using the fitting formula. The fitting formula is as follows.

[0045]

[0046] Where:

[0047] ρ——sulfate ion concentration, mol / L;

[0048] OD 405 ——The coagulation solution absorbs light at a wavelength of 405nm.

[0049] Figure 1 , 2, 3 show that the iron-aluminum double hydroxide and calcium carbonate have obvious visual differences; Figure 5 The maximum concentration of sulfate ions decreased by 0.0246 mol / L. Figure 6It shows that the concentration of sulfate ions decreased by a maximum of 0.0278 mol / L, which indicates that the layered structure of the double metal hydroxide has truly fixed the corrosive ions in the seawater, and the formed products have played a role in repairing cracks and slowing down the expansion damage of concrete.

[0050] Table 1

[0051]

[0052] Table 2

[0053]

Claims

1. Application of a multifunctional color-developing double metal hydroxide for fixing sulfate ions in marine engineering structures, characterized in that: The application method comprises the following steps: (1) preparing a simulated seawater solution, adding a concrete simulated pore solution agent thereto, and mixing them evenly; the ingredients of the concrete simulated pore solution agent are Ca(OH)2, NaOH and KOH; (2) adding a combination of ferrous lactate powder, sodium aluminate powder and calcium nitrite powder to the above mixed solution for reaction to obtain a mixed solution; the masses of the sodium aluminate powder, ferrous lactate powder and calcium nitrite powder are 7.56g, 21.32g, 15.1216g or 8.505g, 23.985g, 17.0118g or 9.45g, 26.65g, 18.902g respectively; (3) Filter the mixture solution to obtain a mixture solid, and dry the solid to obtain a double metal hydroxide having a mixed color of white and brown-red.

2. The use of the multifunctional color-developing double metal hydroxide in fixing sulfate ions in marine engineering structures according to claim 1, characterized in that: The simulated seawater solution in step (1) has a chloride ion concentration of 0.490-0.500 mol / L and a sulfate ion concentration of 0.025-0.035 mol / L.

3. The use of the multifunctional color-developing double metal hydroxide in fixing sulfate ions in marine engineering structures according to claim 1, characterized in that: The solution reaction time in step (2) is 14 to 28 days.

4. The use of the multifunctional color-developing double metal hydroxide in fixing sulfate ions in marine engineering structures according to claim 1, characterized in that: In step (3), the drying temperature is 40-50 °C and the drying time is more than 12 h.

5. The use of the multifunctional color-developing double metal hydroxide in fixing sulfate ions in marine engineering structures according to claim 1, characterized in that: The multifunctional color-developing double metal hydroxide is used for crack repairing, and different types of double metal hydroxides are marked by mixing brown-red and white colors to distinguish the distribution range of the double metal hydroxides.