Two-component coating composition and method for producing coated article

By using a two-component coating composition of polyhydroxy compounds and isocyanurate compounds in open pressurized coating, the problems of solvent scattering and low yield in spraying technology are solved, and high weather resistance and thickness are achieved The formation of coating film improves the performance and production efficiency of the coating product.

CN116367930BActive Publication Date: 2024-11-29NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180074026.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-11-29
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

The existing spraying technology generates solvent scattering and CO2 emissions in the drying process, and the yield is prone to decrease, making it difficult to form a high weather resistance and thick coating film.

Method used

Using a two-component coating composition, including a polyhydroxy compound, an isocyanurate compound and an ultraviolet absorber, a coating film is formed by pressing it under heating conditions by open pressurized coating, reducing solvent content and improving curing efficiency.

Benefits of technology

It is achieved to form a high weather resistance and thick coating film in open pressurized coating, reducing edge collapse and bubble phenomena, improving weather resistance and water resistance of coating products, and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005038502880000271
    Figure GDA0005038502880000271
  • Figure GDA0005038502880000281
    Figure GDA0005038502880000281
  • Figure GDA0005038502880000291
    Figure GDA0005038502880000291
Patent Text Reader

Abstract

The present invention provides a two-component coating composition suitable for open pressure coating and particularly suitable for exterior decoration. A two-component coating composition comprising a main agent and a curing agent, wherein the main agent comprises a polyhydroxy compound, a curing catalyst and an ultraviolet absorber, the curing agent comprises an isocyanurate compound, the polyhydroxy compound has a hydroxyl value of 250 mgKOH / g or more and 1000 mgKOH / g or less, the average number of hydroxyl groups of the polyhydroxy compound is 3 or more, the content of the curing catalyst is 0.05 mass part or more and 3 mass parts or less relative to 100 mass parts of the polyhydroxy compound, and the content of the solvent is 30 mass % or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a two-component coating composition and a method for producing a coated article. Background Art

[0002] A coating film having various functions is formed on the surface of industrial products, etc. The coating film protects the coated object and gives a beautiful appearance and excellent design. The coating film is usually formed by spraying a coating composition containing a solvent such as an organic solvent and / or an aqueous solvent and then drying it. However, in recent years, the scattering of solvents during spraying or the atmospheric emission of solvents in the drying process, the generation of CO2, etc. are considered problems. Moreover, spraying requires a drying process, so the yield is easy to decrease.

[0003] Therefore, as a coating method replacing spray coating, Patent Document 1 proposes a method in which a coating is injected into a mold and then a coating surface is pressed in the mold to form a coating film.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent document 1: International Publication No. 2010 / 113847. Summary of the invention

[0007] Problems to be solved by the invention

[0008] In view of this, the present invention aims to provide a two-component coating composition suitable for open pressure coating (press coating) in which a coating surface is pressed in an open state. In particular, the present invention aims to provide a two-component coating composition suitable for exterior decoration and a method for producing a coated article using the same.

[0009] Means for solving problems

[0010] In order to solve the above-mentioned problems, the present invention provides the following solutions.

[0011] [1] A two-component coating composition comprising a base agent and a curing agent,

[0012] The main agent comprises a polyhydroxy compound, a curing catalyst and an ultraviolet absorber.

[0013] The curing agent comprises an isocyanurate compound,

[0014] The hydroxyl value of the polyol is 250 mgKOH / g or more and 1000 mgKOH / g or less.

[0015] The average number of hydroxyl groups in the polyhydroxy compound is 3 or more.

[0016] The content of the curing catalyst is 0.05 parts by mass or more and 3 parts by mass or less relative to 100 parts by mass of the polyhydroxy compound.

[0017] The content of the solvent is 30% by mass or less.

[0018] [2] The two-component coating composition according to [1] above, wherein the isocyanurate compound comprises a trimer of hexamethylene diisocyanate.

[0019] [3] The two-component coating composition described in [1] or [2] above, wherein the main agent further comprises a light stabilizer.

[0020] [4] The two-component coating composition according to any one of [1] to [3] above, wherein the polyhydroxy compound is at least one selected from polyester polyol, polyether polyol and polycarbonate polyol.

[0021] [5] The two-component coating composition according to any one of [1] to [4] above, wherein the ratio of the isocyanate group equivalent of the isocyanurate compound to the hydroxyl group equivalent of the polyol compound: NCO / OH is greater than 0.5 / 1 and less than 2 / 1.

[0022] [6] The two-component coating composition described in any one of [1] to [5] above, wherein the curing catalyst comprises at least one organic metal catalyst comprising a metal element selected from Bi, Zn, Al, Zr and Sn.

[0023] [7] The two-component coating composition according to any one of [1] to 6] above, which is used for exterior decoration and for open pressure coating.

[0024] [8] A method for producing a coated article, comprising the following steps:

[0025] The process of preparing the object to be coated;

[0026] A step of applying the two-component coating composition described in any one of [1] to [7] above to the object to be coated; and

[0027] A step of pressing the surface of the object to be coated on which the two-component coating composition is applied while heating to cure the two-component coating composition to form a first coating film.

[0028] [9] The method for producing a coated article according to [8] above, wherein the thickness of the first coating film is 80 μm or more.

[0029]

[10] A method for producing a coated article, comprising the following steps:

[0030] The process of preparing an object to be coated with a colored coating film;

[0031] A step of applying the two-component coating composition described in any one of [1] to [7] above onto the colored coating film; and

[0032] A step of pressing the surface of the object to be coated with the two-component coating composition while heating to cure the two-component coating composition to form a second coating film.

[0033]

[11] The method for producing a coated article according to

[10] above, wherein the thickness of the second coating film is 80 μm or more.

[0034] Effects of the Invention

[0035] According to the present invention, a two-component coating composition which is suitable for open pressure coating and particularly suitable for exterior decoration, and a method for producing a coated article using the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] [ Figure 1A ] is a cross-sectional view schematically showing a portion of the coated article involved in the first embodiment.

[0037] [ Figure 1B ] is a cross-sectional view schematically showing a portion of another coated article involved in the first embodiment.

[0038] [ Figure 2 ] is a cross-sectional view schematically showing a portion of the coated article involved in the second embodiment.

[0039] [ Figure 3 ] is a flow chart showing a method for manufacturing a coated article according to one embodiment of the present invention.

[0040] [ Figure 4 ] is a flow chart showing a method for manufacturing a coated article according to another embodiment of the present invention. DETAILED DESCRIPTION

[0041] External decorative paint is a material that forms a coating film on an external decorative body. An external decorative body is a coated body that is mainly used outdoors. Strict weather resistance is required for external decorative bodies. Therefore, light stabilizers and / or ultraviolet absorbers are usually mixed into external decorative paints.

[0042] In order to improve weather resistance, the thickness of the coating film is also important. The thicker the coating film, the higher the weather resistance. Therefore, open pressure coating that can form a thick coating film is focused on. Open pressure coating refers to a method in which after applying a coating on an object, the coating surface is pressed in an open state to form a cured coating film. When the coating contains a thermosetting resin, pressing can be performed simultaneously with heating.

[0043] The two-component coating composition involved in the present embodiment includes: a main agent containing a polyhydroxy compound, a curing catalyst and an ultraviolet absorber; and a curing agent containing an isocyanurate compound. The hydroxyl value of the polyhydroxy compound is greater than 250 mgKOH / g and less than 1000 mgKOH / g, the average number of hydroxyl groups of the polyhydroxy compound is greater than 3, the content of the curing catalyst is greater than 0.05 mass parts and less than 3 mass parts relative to 100 mass parts of the polyhydroxy compound, and the content of the solvent is less than 30 mass%. While the two-component coating composition exhibits excellent weather resistance and water resistance, it is not easy to collapse or bubble even when a thick coating film is formed. Therefore, the two-component coating composition involved in the present embodiment is for open pressure coating and is particularly suitable for use as exterior decoration.

[0044] However, the two-component coating composition according to the present embodiment does not exclude the use in coating methods other than open press coating.

[0045] The two-component coating composition according to the present embodiment can be used as a material for a coating film (first coating film) disposed adjacent to a coating object and a coating film (second coating film) disposed adjacent to a colored coating film formed on the coating object.

[0046] [Two-component coating composition]

[0047] The two-component coating composition involved in the present embodiment comprises a main agent and a curing agent. The main agent comprises a polyol, a curing catalyst and an ultraviolet absorber. The curing agent comprises an isocyanurate compound. By mixing the main agent and the curing agent, the polyol reacts with the isocyanurate compound to obtain a cured coating film. The main agent and / or the curing agent can be heated and / or vacuum degassed before mixing, respectively. Thus, the amount of water contained in the two-component coating composition obtained by mixing the two decreases, and the appearance of the obtained coating film is easily improved.

[0048] (Main agent)

[0049] The main agent includes a polyhydroxy compound, a curing catalyst and an ultraviolet absorber. The polyhydroxy compound is a film-forming resin. The polyhydroxy compound reacts with a curing agent, for example, by heating to form a three-dimensional cured film. Hereinafter, the curable resin containing the polyhydroxy compound contained in the two-component coating composition is sometimes collectively referred to as a film-forming resin.

[0050] Hereinafter, each component will be described in detail.

[0051] 《UV absorber》

[0052] Ultraviolet light absorbers (UVA) absorb ultraviolet light and prevent the coating from deteriorating due to ultraviolet light. Therefore, they are particularly suitable for clear coatings.

[0053] Examples of UVA include benzotriazole compounds, triazine compounds, benzophenone compounds, and benzoate compounds. Specific examples of UVA include Tinuvin 326, Tinuvin 384-2, Tinuvin 900, Tinuvin 400, Tinuvin 405, Tinuvin 460, Tinuvin 477, and Tinuvin 479 (all manufactured by BASF).

[0054] The content of UVA (PHR: mass %) relative to 100 mass % of the resin solid content of the coating composition is, for example, 0.2 mass % or more and 10 mass % or less. The PHR of UVA is more preferably 1 mass % or more, and further preferably 2 mass % or more. The PHR of UVA is more preferably 7 mass % or less, and further preferably 5 mass % or less.

[0055] Light stabilizer

[0056] The ultraviolet absorber can be used together with the light stabilizer. As a result, the weather resistance is easily further improved. The light stabilizer efficiently captures the alkyl radicals (R·) or peroxide radicals (ROO·) generated by ultraviolet rays. Examples of the light stabilizer include hindered amine compounds (HALS) and hindered phenol compounds. Among them, HALS is preferred.

[0057] The structure of HALS is not particularly limited. HALS has, for example, one or more piperidine skeletons (typically, 2,2,6,6-tetraalkylpiperidine skeletons) in the molecule. Such HALS may be used alone or in combination of two or more.

[0058] The nitrogen atom of the hindered amino group constituting the HALS (typically, the nitrogen atom of the piperidine skeleton) may be bonded to hydrogen (NH type), may be bonded to an alkyl group (NR type), may have an ether bond (N-OR type), may have a hydroxyl group via an ether bond (N-OR-OH type), or may be bonded to an acyl group (N-CO-R type). Among them, the hindered amino group is preferably of N-OR type and N-CO-R type.

[0059] There is no particular limitation on the molecular weight of the light stabilizer. Among them, the molecular weight of the light stabilizer is preferably 400 or more and 800 or less. As a result, it is easy to improve the compatibility with polyhydroxy compounds. Moreover, it is also easy to suppress the dissolution or bleeding of the light stabilizer from the coating film. The molecular weight of the light stabilizer is more preferably 410 or more, and further preferably 420 or more. In the case where the light stabilizer does not have a hydroxyl group in the molecule, the molecular weight of the light stabilizer is more preferably 700 or less, and further preferably 600 or less. Even if the molecular weight of the light stabilizer having a hydroxyl group is large, the compatibility with the polyhydroxy compound is high. Therefore, the upper limit value of the molecular weight of the HALS having a hydroxyl group can be 790 or 780.

[0060] In addition, HALS having a hydroxyl group is also preferred in that it is not easy to dissolve or bleed out from the coating film. HALS having a large molecular weight is generally easy to dissolve or bleed out from the coating film. However, HALS having a hydroxyl group can react with a curing agent, so it is easy to suppress dissolution or bleed out from the coating film even if it has a large molecular weight.

[0061] Preferred HALS include, specifically, HOSTAVIN (registered trademark) 3058 (manufactured by Clariant Chemicals, molecular weight 449, N-CO-R type), Tinuvin (registered trademark) 123 (hereinafter, manufactured by BASF, molecular weight 737, N-OR type), Tinuvin 152 (molecular weight 757, N-OR type), and Tinuvin 5100.

[0062] Specific examples of preferred hindered phenol-based light stabilizers include Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1726, Irganox 1035, Irganox 1076, Irganox 1135, and Irganox 1726 (all manufactured by BASF Corporation).

[0063] The content of the light stabilizer (PHR: mass %) is preferably 0 mass % or more and less than 5 mass % relative to the resin solid content of the coating composition. The PHR of the light stabilizer is more preferably 0.5 mass % or more, and further preferably 1 mass % or more. The PHR of the light stabilizer is more preferably 4 mass % or less, and further preferably 3 mass % or less. Among the light stabilizers, neutral HALS preferably accounts for 50 mass % or more, and preferably 70 mass % or more. The resin solid content of the coating composition refers to the total solid content of the coating film forming resin and the curing agent. PHR is the ratio relative to 100 mass % of the above-mentioned resin solid content.

[0064] Polyhydroxy compounds

[0065] The polyol is a coating film forming resin. The polyol forms a three-dimensional cured coating film by, for example, reacting with a curing agent by heating. Each molecule of the polyol has two or more hydroxyl groups. In the present embodiment, the main agent contains a polyol having an average of more than three hydroxyl groups per molecule. Thus, the hardness of the obtained coating film is improved. The polyol can be used alone or in combination of two or more.

[0066] The main agent preferably comprises a polyhydroxy compound (A1) having three or more hydroxyl groups per molecule and a polyhydroxy compound (A2) having two hydroxyl groups per molecule. The ratio of the polyhydroxy compound (A1) to the polyhydroxy compound (A2) is not particularly limited. The ratio of the polyhydroxy compound (A2) may be less than 50% by mass, less than 40% by mass, or less than 30% by mass of the total of the polyhydroxy compound (A1) and the polyhydroxy compound (A2).

[0067] The hydroxyl value of the polyol is 250 mgKOH / g or more and 1000 mgKOH / g or less. By making the hydroxyl value of the polyol within the above range, when the main agent and the curing agent are mixed, the reaction rate of the polyol and the isocyanate compound increases. Therefore, the coated product can be quickly demolded from the mold, and the yield is improved. In addition, a certain degree of reaction heat is generated during the reaction, so the adhesion between the coating film and the resin coated object is particularly easy to improve.

[0068] When two or more polyhydroxy compounds are included, the apparent hydroxyl value calculated based on the hydroxyl value and mass ratio of each polyhydroxy compound can be 250 mgKOH / g or more and 1000 mgKOH / g or less. That is, the main agent can include a polyhydroxy compound having a hydroxyl value of less than 250 mgKOH / g and / or a polyhydroxy compound having a hydroxyl value of more than 1000 mgKOH / g.

[0069] The hydroxyl value (including apparent hydroxyl value, hereinafter the same) of the polyol is preferably 350 mgKOH / g or more, more preferably 500 mgKOH / g or more. The hydroxyl value of the polyol is preferably 800 mgKOH / g or less, more preferably 700 mgKOH / g or less.

[0070] There is no particular limitation on the type of polyhydroxy compound. Examples of the polyhydroxy compound include polyester polyols, polyether polyols, polycarbonate polyols, polyacrylate polyols, and polyols. These can be used alone or in combination of two or more. The polyhydroxy compound preferably includes at least one selected from polyester polyols, polyether polyols, and polycarbonate polyols.

[0071] The polyester polyol preferably has a branched structure. The polyester polyol having a branched structure can be prepared by, for example, reacting a divalent or higher polycarboxylic acid with a trivalent or higher polyol compound, and repeating the above reaction as necessary.

[0072] Examples of commercially available polyester polyols include Desmophen VPLS2249 / 1 (manufactured by Sumika Covestro Urethane Co., Ltd.), Desmophen 800 (manufactured by Sumika Covestro Urethane Co., Ltd.), Desmophen XP2488 (manufactured by Sumika Covestro Urethane Co., Ltd.), Kuraray Polyol P-510 (manufactured by Kuraray Co., Ltd.), and Kuraray Polyol F-510 (manufactured by Kuraray Co., Ltd.).

[0073] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and their block products. Polyether polyols can be prepared by adding ethylene oxide and / or propylene oxide to polyol compounds. By the above steps, polyether polyols having a divalent, trivalent, or higher number of OH functional groups per molecule can be prepared.

[0074] Examples of commercially available products of polyether polyols include the SANNIX series manufactured by Sanyo Chemical Industries, Ltd. Specifically, SANNIX GP-250, SANNIX GP-400, SANNIX PP-200, and SANNIX GP-600 may be mentioned.

[0075] The polycarbonate polyol can be prepared by, for example, reacting dimethyl carbonate with a polyhydric alcohol.

[0076] Examples of commercially available products of the polycarbonate polyol include Duranol T5650E (manufactured by Asahi Kasei Corporation), C-590 (manufactured by Kuraray Corporation), and ETERNACOLL PH-50 (manufactured by Ube Industries, Ltd.).

[0077] Examples of the polyol include ethylene glycol, glycerin, trimethylolpropane, propylene glycol, butanediol (tetramethylene glycol), and pentaerythritol.

[0078] The weight average molecular weight (Mw) of the polyhydroxy compound is not particularly limited, and the Mw of the polyhydroxy compound can be appropriately set according to the hydroxyl value and the like.

[0079] The main agent may contain other film-forming resins other than the polyol compound. Examples of the film-forming resin include acrylic resins, polyester resins, alkyd resins, polyether resins, polyolefin resins, polyurethane resins, polycarbonate resins, melamine resins, epoxy resins, and carbodiimide resins. Other film-forming resins may be used alone or in combination of two or more.

[0080] 《Curing Catalyst》

[0081] The curing catalyst promotes the curing reaction. There is no particular limitation on the curing catalyst. From the viewpoint of the promoting effect, the curing catalyst is preferably at least one organic metal catalyst, which contains a metal element selected from Bi, Zn, Al, Zr and Sn.

[0082] Examples of organic metal catalysts containing Bi include bismuth carboxylic acids and salts thereof. Examples of organic metal catalysts containing Zn include zinc complex catalysts. Examples of organic metal catalysts containing Al include aluminum complex catalysts. Examples of organic metal catalysts containing Zr include zirconium chelate catalysts. Examples of organic metal catalysts containing Sn include dialkyltin dicarboxylates such as dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin diacetate; tin oxide compounds such as dibutyltin oxide; and tin carboxylates such as tin 2-ethylhexanoate.

[0083] Examples of commercially available organometallic catalysts containing Bi include K-KAT 348 (manufactured by Kusumoto Chemicals, Ltd.) and K-KAT XK-640 (manufactured by Kusumoto Chemicals, Ltd.). Examples of commercially available organometallic catalysts containing Zr include K-KAT 4205, K-KAT XC-9213, K-KAT XC-A209, and K-KAT 6212 (manufactured by Kusumoto Chemicals, Ltd.). Examples of commercially available organometallic catalysts containing Al include K-KAT 5218 (manufactured by Kusumoto Chemicals, Ltd.). Examples of commercially available organometallic catalysts containing Zn include K-KAT XK-314, K-KATXK-635, K-KAT XK-639, and K-KAT XK-620 (manufactured by Kusumoto Chemicals, Ltd.). Examples of commercially available products of the Sn-containing organic metal catalyst include TVS TIN LAU (manufactured by Nitto Kasei Co., Ltd.).

[0084] Relative to 100 parts by mass of the film-forming resin, the content of the curing catalyst is, for example, 0.05 parts by mass or more and 3 parts by mass or less. Thus, the curing reaction of the film-forming resin is rapidly carried out. Thus, by open pressure coating, a film having excellent appearance and physical properties can be obtained. Relative to 100 parts by mass of the film-forming resin, the content of the curing catalyst is preferably 0.07 parts by mass or more, more preferably 0.1 parts by mass or more. Relative to 100 parts by mass of the film-forming resin, the content of the curing catalyst is preferably 1 parts by mass or less, more preferably 0.7 parts by mass or less.

[0085] (Curing agent)

[0086] By crosslinking the coating film-forming resin such as a polyol with a curing agent, the corrosion resistance and durability of the resulting coating film are improved.

[0087] The curing agent contains an isocyanurate compound. The isocyanurate compound is a trimer of an isocyanate compound and has a ring structure. The isocyanurate compound further improves the curability of the polyol compound and improves weather resistance.

[0088] The isocyanate compound is not particularly limited, and a substance known as a curing agent for a two-component reactive composition can be used. Examples of the isocyanate compound include aromatic diisocyanates such as toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI), and meta-xylylene diisocyanate (MXDI); aliphatic diisocyanates such as hexamethylene diisocyanate (HDI), tetramethylene diisocyanate, 2-methyl-pentane-1,5-diisocyanate, 3-methyl-pentane-1,5-diisocyanate, lysine diisocyanate, and trioxyethylene diisocyanate; and alicyclic diisocyanates such as isophorone diisocyanate (IPDI), cyclohexyl diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, norbornane diisocyanate, hydrogenated toluene diisocyanate, hydrogenated xylene diisocyanate, and hydrogenated tetramethylxylene diisocyanate. These may be used alone or in combination of two or more.

[0089] Among them, aliphatic diisocyanates are preferred, and HDI is more preferred, in terms of lower viscosity. The trimers of these isocyanates are particularly reactive with polyols, and therefore are more suitable for open pressure coating.

[0090] The ratio of the isocyanate group equivalent of the isocyanate compound to the hydroxyl group equivalent of the polyol compound: NCO equivalent / OH equivalent is preferably 0.5 / 1 to 2 / 1, more preferably 0.9 / 1 to 1.2 / 1. When the equivalent ratio is within the above range, the curability is high and it is particularly suitable for open pressure coating.

[0091] The curing agent may include other curing agents other than the isocyanurate compound. As other curing agents, for example, amino resins, monomers or dimers of the above-mentioned isocyanate compounds, biuret bodies of the above-mentioned isocyanate compounds, blocked products of the above-mentioned isocyanate compounds, epoxy compounds, aziridine compounds, carbodiimide compounds, and oxazoline compounds can be cited. These can be used alone or in combination of two or more.

[0092] The content of the curing agent is, for example, 35% by mass or more and 90% by mass or less of the resin solid content of the coating composition. The above-mentioned content of the curing agent is preferably 45% by mass or more, more preferably 55% by mass or more. The above-mentioned content of the curing agent is preferably 85% by mass or less, more preferably 70% by mass or less.

[0093] (Solvent)

[0094] The content of the solvent is 30% by mass or less. Thus, a cured coating can be obtained quickly. Thus, by open pressure coating, a coating with excellent appearance and physical properties can be obtained. The content of the solvent is preferably 10% by mass or less, and can be 0%.

[0095] There is no particular limitation on the solvent. The solvent is usually an organic solvent. Examples of the organic solvent include ester solvents such as ethyl acetate, butyl acetate, isopropyl acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; ether solvents such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, methyl methoxybutanol, ethoxypropanol, ethylene glycol isopropyl ether, ethylene glycol-tert-butyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, methoxybutanol, and propylene glycol monobutyl ether; alcohol solvents such as methanol, ethanol, butanol, and propanol; ketone solvents such as acetone, butanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as Swazol, SHELLSOL, and mineral spirit; aromatic solvents such as xylene, toluene, Solvesso-100 (S-100), and Solvesso-150 (S-150). These can be used alone or in combination of two or more.

[0096] "pigment"

[0097] The main agent may contain a pigment. Examples of the pigment include coloring pigments, bright pigments, and extender pigments. The pigment may be used alone or in combination of two or more.

[0098] Examples of the bright pigment include metal flakes (aluminum, chromium, gold, silver, copper, brass, titanium, nickel, nickel-chromium, stainless steel, etc.), metal oxide flakes, pearlescent pigments, glass flakes coated with metals or metal oxides, silicon dioxide flakes coated with metal oxides, graphite, holographic pigments, and cholesteric liquid crystal polymers. These can be used alone or in combination of two or more.

[0099] Examples of coloring pigments include organic coloring pigments such as azo chelate pigments, insoluble azo pigments, condensed azo pigments, diketopyrrolopyrrole pigments, benzimidazolone pigments, phthalocyanine pigments, indigo pigments, perinone pigments, perylene pigments, dioxane pigments, quinacridone pigments, isoindolinone pigments, and metal complex pigments; and inorganic coloring pigments such as chrome yellow, yellow iron oxide, red iron oxide, carbon black, and titanium dioxide. These can be used alone or in combination of two or more.

[0100] Examples of the extender pigment include calcium carbonate, barium sulfate, clay, and talc, and these may be used alone or in combination of two or more.

[0101] There is no particular limitation on the content of the pigment. The content of the pigment can be appropriately set according to its type or purpose. For example, a coating main agent that requires transparency may contain a pigment within a range that does not impair transparency. In a coating main agent that requires transparency, the amount of pigment added is, for example, 10 parts by mass or less, and can be 0.01 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the solid content of the coating film-forming resin. In an opaque coating main agent, the amount of pigment added may, for example, exceed 10 parts by mass relative to 100 parts by mass of the solid content of the coating film-forming resin.

[0102] Viscosity Regulator

[0103] The main agent may contain a viscosity adjuster. Examples of the viscosity adjuster include amide-based adhesives, inorganic adhesives, cellulose derivatives, and urethane associative adhesives. These may be used alone or in combination of two or more.

[0104] Examples of the amide viscosity adjuster include fatty acid amide, polyamide, acrylamide, long-chain polyaminoamide, aminoamide, and salts thereof (eg, phosphates).

[0105] Examples of the inorganic binder include layered silicates (silicate minerals), halogenated minerals, oxide minerals, carbonate minerals, borate minerals, sulfate minerals, molybdate minerals, tungstate minerals, phosphate minerals, arsenate minerals, and vanadate minerals.

[0106] As a cellulose derivative, cellulose acetate butyrate, nitrocellulose, cellulose acetate, and cellulose acetate propionate are mentioned, for example.

[0107] The urethane associative adhesive is not particularly limited. Examples of the urethane associative adhesive include polyurethane adhesives having a hydrophobic chain in the molecule and urethane-urea adhesives having at least a portion of a main chain being a hydrophobic urethane chain.

[0108] (other)

[0109] The two-component coating composition may contain other ingredients as required. As other ingredients, for example, additives commonly used in the coating field and the coating field can be cited. Specifically, various pigments, surface conditioning agents, viscosity regulators, antioxidants, UV protection agents, defoamers, catalyst promoters, rust inhibitors, anti-settling agents, dispersants, etc. can be cited. These additives can be added to the main agent or to the curing agent. The amount of the additive is not particularly limited and can be appropriately set as required.

[0110] [Painted items]

[0111] (First embodiment)

[0112] The coated article involved in the first embodiment comprises a coated article and a first coating film formed on the coated article. The first coating film is formed by the above-mentioned two-component coating composition. In addition, the first coating film is formed by open pressure coating. The thickness of the first coating film is preferably 80 μm or more. The coated article preferably includes a fiber-reinforced resin substrate.

[0113] The first coating film can function as a clear coating film, a primer coating film, a so-called intermediate coating film, and a base coating film. The first coating film may be transparent or opaque.

[0114] Transparency specifically means that the total light transmittance is 80% or more. The total light transmittance of the transparent coating is preferably 90% or more. Opaque specifically means that the total light transmittance is less than 80%. The total light transmittance can be measured by a method based on JIS K 7361-1. The transparent coating can be colorless or colored.

[0115] Another coating film may be further formed on the first coating film. For example, the other coating film is at least one selected from a mid-coat coating film, a primer coating film, and a clear coating film. The other coating film is formed by a coating other than the above-mentioned two-component coating composition by a method other than open pressure coating (representatively spraying).

[0116] (Second embodiment)

[0117] The coated article involved in the second embodiment comprises: a coated object, a colored coating film formed on the coated object, and a second coating film formed on the colored coating film. The second coating film is formed by the above-mentioned two-component coating composition. In addition, the second coating film is formed by open pressure coating. The thickness of the second coating film is preferably 80 μm or more.

[0118] The second coating film can function as a top clear coating film. The second coating film preferably has transparency.

[0119] The colored coating film includes a so-called intermediate coating film and a primer coating film. The colored coating film is formed by a coating material other than the above-mentioned two-component coating composition and by a method other than open pressure coating (typically, spray coating).

[0120] (1st and 2nd coating)

[0121] The thickness of the first and second coating films is, for example, more than 80 μm. Thus, the weather resistance of the coated article is more easily improved. According to the two-component coating composition involved in the present embodiment, even such a thick coating film can be made into a film while suppressing edge collapse or blistering. Moreover, even if the surface of the coated object has concavoconvexities such as fiber reinforced resin (FRP), in addition, even if the surface of the colored coating film has concavoconvexities formed by coloring pigments, these concavoconvexities are not easy to appear on the surface of the first and second coating films. Therefore, the pattern of the pressing member can be transferred with high precision on the surface of the first and second coating films formed by open pressure coating. For example, when the pressing surface of the pressing member is a mirror surface, a smooth and glossy first and second coating film can be obtained. The thickness of the first and second coating films is more preferably more than 85 μm, and more preferably more than 150 μm. The thickness of the first and second coating films can be less than 1000 μm.

[0122] The thickness of the first and second coatings can be calculated, for example, as follows. First, each coating is cut out together with the coated object using a carving knife or the like. A slice having a vertical cross section is then obtained from the cut sample using a blade or a slicer. The slice is observed under a video microscope (e.g., VHX-6000, manufactured by KEYENCE) to measure the coating thickness at any five points. Finally, these measured values ​​are averaged as the coating thickness. The thickness of other coatings is also measured and calculated in the same manner.

[0123] (Object to be coated)

[0124] The object to be coated is not particularly limited and may be made of, for example, metal, resin, or glass.

[0125] Examples of the metal material constituting the metal coating object include iron, copper, aluminum, tin, zinc, and alloys thereof.

[0126] The metal object to be coated may be subjected to surface treatment. Examples of the surface treatment include phosphate treatment, chromate treatment, zirconium treatment, and composite oxide treatment. The metal object to be coated may be further coated with an electrodeposition coating after the surface treatment. The electrodeposition coating may be a cationic or anionic type.

[0127] The resin constituting the resin-made coated object may be a thermoplastic resin or a thermosetting resin. Examples of these resins include polypropylene (PP) resin, acrylonitrile / butadiene / styrene copolymer (ABS resin), polycarbonate (PC) / ABS resin, PC / acrylonitrile / ethylene-propylene-diene / styrene copolymer (AES resin), AES resin, PC / polybutylene terephthalate (PBT) resin, PC / polyethylene terephthalate (PET) resin, PC resin, polymethyl methacrylate (PMMA) resin, polyvinyl chloride (PVC resin), acrylonitrile / styrene / acrylic acid (ASA) resin, epoxy resin, and phenolic resin.

[0128] From the viewpoint of design, the resin coated object can be a fiber reinforced resin (FRP) substrate containing both resin and fiber. As the fiber contained in the FRP substrate, for example, carbon fiber and glass fiber can be cited. According to the two-component coating composition involved in this embodiment, a thick coating film can be formed, so the unevenness of the FRP substrate can be concealed. From the viewpoint of design, a fiber reinforced resin (CFRP) substrate containing carbon fiber is particularly preferred.

[0129] The resin substrate is preferably subjected to a degreasing treatment. After the degreasing treatment, the resin substrate may be further coated with a primer. The primer is not particularly limited and may be appropriately selected according to the type of coating to be applied thereon.

[0130] (Colored coating)

[0131] The colored coating film may be a single layer or a laminated coating film of two or more layers. The colored coating film may be a so-called intermediate coating film of one or more layers, a so-called primer coating film of one or more layers, or a combination thereof.

[0132] 《Base coating film》

[0133] The primer coating film is formed by a primer coating composition comprising a film-forming resin, a curing agent, a viscosity modifier, a diluent component and a pigment. The primer coating composition may include various additives as required. The components contained in each primer coating film may be the same or different.

[0134] Examples of the coating film-forming resin, curing agent, viscosity adjuster, diluent component and pigment include the components exemplified as components to be blended in the two-component coating composition. The diluent component may be water.

[0135] The thickness of the primer coating film is not particularly limited and is appropriately set according to the purpose. The thickness of each layer of the primer coating film can be, for example, 15 μm or more and 50 μm or less. The thickness of each layer of the primer coating film is preferably 18 μm or more, more preferably 20 μm or more. The thickness of each layer of the primer coating film is preferably 45 μm or less, more preferably 40 μm or less.

[0136] 《Middle coating film》

[0137] The intermediate coating film usually exists between the object to be coated and the base coating film. The intermediate coating film makes the coating surface uniform and it is easy to suppress the unevenness of the base coating film.

[0138] The mid-coat film is formed of, for example, a mid-coat composition containing a film-forming resin, a curing agent, a viscosity modifier, a diluent component, and a pigment. The mid-coat composition may contain various additives as necessary.

[0139] Examples of the coating film-forming resin, curing agent, viscosity adjuster, diluent component and pigment include the components exemplified as components to be blended in the two-component coating composition. The diluent component may be water.

[0140] There is no particular limitation on the thickness of the mid-coat film. In terms of the appearance and chipping resistance of the coated article, the thickness of the mid-coat film is preferably 10 μm or more and 40 μm or less. The thickness of the mid-coat film is more preferably 15 μm or more. The thickness of the mid-coat film is more preferably 30 μm or less.

[0141] 《Transparent coating》

[0142] The transparent coating film protects the lower coating film and brings a glossy or matte texture to the coated article. The transparent coating film is not particularly limited and has the same structure as the transparent coating films known in the past. The transparent coating film is formed, for example, by a transparent coating composition comprising a coating film forming resin, a curing agent, a viscosity modifier, a diluting component and a pigment. The transparent coating composition may contain various additives as needed.

[0143] Examples of the coating film-forming resin, curing agent, viscosity adjuster, diluent component and pigment include the components exemplified as components to be blended in the two-component coating composition. The diluent component may be water.

[0144] The thickness of the transparent coating film is not particularly limited. From the viewpoint of scratch resistance, the thickness of the transparent coating film is preferably 10 μm or more, more preferably 15 μm or more. From the viewpoint of design, the thickness of the transparent coating film may be 50 μm or less, or 40 μm or less.

[0145] Figure 1A1 is a cross-sectional view schematically showing a portion of a coated article according to the first embodiment. The coated article 100A includes a coated article 10 and a first coating film 20A. The coated article 10 includes, for example, a CFRP substrate, and has irregularities from carbon fibers formed on its surface. On the other hand, the surface of the first coating film 20A does not show the irregularities, and the surface of the coated article 100A is smooth.

[0146] Figure 1B It is a cross-sectional view schematically showing a part of another coated article involved in the first embodiment. The coated article 100B comprises: an object to be coated 10, a first coating film 20A, and another coating film 30 formed on the first coating film 20A. The other coating film 30 comprises a primer coating film 31 and a transparent coating film 32. The object to be coated 10, for example, includes a CFRP substrate, and the surface thereof has irregularities from carbon fibers. On the other hand, the above-mentioned irregularities are not shown on the surfaces of the first coating film 20A and the other coating film 30, and the surface of the coated article 100A is smooth.

[0147] Figure 2 2 is a cross-sectional view schematically showing a portion of a coated article according to the second embodiment. The coated article 200 comprises: an object to be coated 10, a color coating film 40, and a second coating film 20B. The object to be coated 10, for example, includes a CFRP substrate, and the surfaces of the object to be coated 10 and the color coating film 40 are formed with irregularities from carbon fibers. On the other hand, the surface of the second coating film 20B does not show the irregularities, and the surface of the coated article 200 is smooth.

[0148] [Method for producing coated article]

[0149] The coated article involved in the first embodiment is manufactured by a method comprising the following steps: a step of preparing a coated object; a step of applying the above-mentioned two-component coating composition on the coated object; and a step of heating and pressing the coated surface of the coated object to cure the two-component coating composition to form a first coating film.

[0150] The coated article involved in the second embodiment is manufactured by a method comprising the following steps: a step of preparing a coated object having a colored coating film; a step of applying the above-mentioned two-component coating composition on the colored coating film; and a step of heating and pressing the coated surface of the coated object to cure the two-component coating composition to form a second coating film.

[0151] The process of applying the two-component coating composition and the process of pressing the coated surface of the object to be coated while heating to form a coating film are also collectively referred to as open pressure coating. Open pressure coating is particularly suitable for coating FRP substrates.

[0152] Hereinafter, a method for producing a coated article according to the first embodiment will be described.

[0153] Figure 3 1 is a flowchart showing a method for producing a coated article according to the first embodiment. (I) Step of Preparing an Article to be Coated (S11)

[0154] First, a coating object is prepared as a coating target. The details of the coating object are as described above. (II) Step of applying the two-component coating composition on the coating object (S12)

[0155] The coating method is not particularly limited and examples of the coating method include dip coating, air knife coating, curtain coating, roll coating, bar coating (eg wire bar coating), die coating, gravure coating and doctor blade coating.

[0156] The coating amount of the two-component coating composition is not particularly limited. The two-component coating composition is applied so that the thickness of the first coating film (coating layer after curing) becomes 80 μm or more.

[0157] From the viewpoint of operability, the viscosity of the two-component coating composition is preferably 100 mPa·s or more and 500 mPa·s or less. Such viscosity can be appropriately adjusted by using the above two-component coating composition. It should be noted that, as required, the main agent and / or curing agent of the two-component coating composition can be heated to adjust to the above viscosity range.

[0158] After applying the two-component coating composition, pre-drying may be performed. The pre-drying conditions are not particularly limited. Examples of pre-drying include a method of leaving the coating at a temperature of 20° C. to 25° C. for 15 minutes to 30 minutes, and a method of heating the coating at a temperature of 50° C. to 100° C. for 30 seconds to 10 minutes.

[0159] (III) Step of pressing the coated surface (S13)

[0160] The coated surface of the object to be coated is pressed while being heated. Thus, the two-component coating composition is cured to obtain a first coating film.

[0161] According to the open pressure coating, a thick first coating film which suppresses edge collapse or blistering can be formed. Therefore, even if the coating is applied to a coated object having a surface with uneven surfaces such as FRP, the uneven surfaces are not easily visible on the coated surface. Therefore, the pattern of the pressing member can be transferred with high precision on the surface of the first coating film formed by the open pressure coating. In addition, since the amount of solvent contained in the two-component coating composition is small, there is no need for a drying process for removing the solvent, and the yield is improved.

[0162] There is no particular limitation on the method of heating the coated surface. For example, the coating surface can be heated by pressing it with a heated pressing member. The heating conditions are appropriately set according to the composition of each coating, etc. The heating temperature is, for example, 80°C to 180°C, and can be 120°C to 160°C. The heating time can be appropriately set according to the heating temperature. When the heating temperature is 120°C to 160°C, the heating time is, for example, 1 minute to 30 minutes, and can be 5 minutes to 20 minutes. There is no particular limitation on the pressing conditions.

[0163] (IV) Step of forming another coating film on the first coating film (S14)

[0164] Other coatings may be formed on the first coating. The other coatings are, for example, at least one selected from a mid-coating, a primer, and a clear coating. From the viewpoint of productivity, adhesion, and water resistance, it is preferred that a plurality of other coatings are laminated without being cured and then heated so that the plurality of uncured coatings are cured simultaneously.

[0165] (IV-1) Step of forming an uncured intermediate coating film

[0166] The uncured mid-coat coating film is formed by applying a mid-coat coating material comprising the above-mentioned mid-coat coating composition.

[0167] There is no particular limitation on the coating method. Examples of coating methods include air spraying, airless spraying, rotary atomization, and curtain coating. These methods can be combined with electrostatic coating. Among them, from the viewpoint of coating efficiency, rotary atomization electrostatic coating is preferred. In rotary atomization electrostatic coating, for example, a rotary atomization electrostatic coating machine commonly known as "micro micro bell (μμbell)", "micro bell (μbell)", "metallic bell (metabell)" or the like is used.

[0168] The amount of the mid-coat paint applied is not particularly limited. The mid-coat paint is applied, for example, so that the thickness of the mid-coat film after curing is 10 μm or more and 40 μm or less.

[0169] After the mid-coat is applied, pre-drying (also called preheating) can be performed. Thus, the dilution components contained in the mid-coat are suppressed from boiling during the curing process, and the generation of bubbles is easily suppressed. Moreover, by pre-drying, the uncured mid-coat film and the coating applied thereon are suppressed from mixing with each other, and it is difficult to form a mixed phase. Therefore, the appearance of the obtained coated article is easily improved.

[0170] The pre-drying conditions are not particularly limited. Examples of pre-drying include a method of leaving the mixture at a temperature of 20°C to 25°C for 15 minutes to 30 minutes, and a method of heating the mixture at a temperature of 50°C to 100°C for 30 seconds to 10 minutes.

[0171] (Mid-coat paint)

[0172] The mid-coat coating comprises the mid-coat coating composition described above. The mid-coat coating can be prepared by further diluting the mid-coat coating composition described above with a diluent component. The mid-coat coating can be a single-component coating or a multi-component coating such as a two-component coating.

[0173] The viscosity of the mid-coat is not particularly limited. The viscosity of the mid-coat measured at 20° C. using a B-type viscometer is, for example, 500 cps / 6 rpm or more and 6000 cps / 6 rpm or less.

[0174] The solid content of the mid-coat is not particularly limited. The solid content of the mid-coat is preferably 30% by mass or more and 70% by mass or less. The solid content of the mid-coat refers to all components excluding dilution components from the mid-coat.

[0175] (IV-2) Step of forming an uncured primer film

[0176] The uncured primer coating film is formed by applying a primer coating material comprising the above-mentioned primer coating composition.

[0177] The coating method is not particularly limited. Examples of the coating method include the same method as the coating method for the mid-coat. Among them, rotary atomization electrostatic coating is preferred from the viewpoint of coating efficiency.

[0178] The amount of primer coating applied is not particularly limited. The primer coating is applied, for example, so that the thickness of the primer coating film after curing is 15 μm or more and 50 μm or less.

[0179] After the primer is applied, it may be pre-dried. The pre-drying conditions are not particularly limited and may be the same as those for the mid-coat.

[0180] (Primer coating)

[0181] The primer coating comprises the above-mentioned primer coating composition. The primer coating can be prepared by further diluting the above-mentioned primer coating composition with a diluent component. The primer coating can be a single-component coating or a multi-component coating such as a two-component coating.

[0182] The viscosity of the primer coating is not particularly limited. The viscosity of the primer coating measured at 20° C. using a B-type viscometer is, for example, 500 cps / 6 rpm or more and 6000 cps / 6 rpm or less.

[0183] The solid content ratio of the primer is not particularly limited. The solid content ratio of the primer is preferably 30% by mass or more and 70% by mass or less. The solid content of the primer refers to all components after removing the dilution components from the primer.

[0184] (IV-3) Step of forming an uncured clear coating film

[0185] The uncured clear coating film is formed by applying a clear coating comprising the above-mentioned clear coating composition.

[0186] The coating method is not particularly limited. Examples of the coating method include the same method as the coating method for the mid-coat. Among them, rotary atomization electrostatic coating is preferred from the viewpoint of coating efficiency.

[0187] The amount of the clear coating material applied is not particularly limited. The clear coating material is applied, for example, so that the thickness of the clear coating film after curing is 25 μm or more and 45 μm or less.

[0188] (Clear coating)

[0189] The clear coating comprises the clear coating composition described above. The clear coating can be prepared by further diluting the clear coating composition described above with a diluent component. The clear coating can be a powder, water-based, or solvent-based.

[0190] The viscosity of the clear coating is not particularly limited. The viscosity of the clear coating measured at 20° C. by a B-type viscometer is, for example, 500 cps / 6 rpm or more and 6000 cps / 6 rpm or less.

[0191] The solid content of the clear coating is not particularly limited. The solid content of the clear coating is, for example, 40% by mass or more and 60% by mass or less. The solid content of the clear coating refers to all components excluding dilution components from the clear coating.

[0192] (IV-4) Curing Step

[0193] At least one selected from the uncured intermediate coating film, the base coating film, and the clear coating film is cured. The curing is performed by heating.

[0194] The heating conditions are appropriately set according to the composition of each coating film, etc. The heating temperature is, for example, 70° C. to 150° C., and may be 80° C. to 140° C. The heating time is, for example, 10 minutes to 40 minutes, and may be 20 minutes to 30 minutes. Examples of the heating device include drying furnaces such as hot air furnaces, electric furnaces, and infrared induction heating furnaces.

[0195] Next, a method for producing a coated article according to a second embodiment will be described.

[0196] Figure 4 1 is a flowchart showing a method for producing a coated article according to the second embodiment. (I) Step of Preparing an Article to be Coated Having a Colored Coating Film (S21)

[0197] The object to be coated has a colored coating film. As described above, the colored coating film is formed, for example, by a method comprising the following steps: a step of applying a mid-coat coating material to the object to be coated to form an uncured mid-coat coating film; a step of applying a primer coating material to form an uncured primer coating film; and a step of curing the two uncured coating films. The two coating films may be cured together with the two-component coating composition. (II) Step of applying the two-component coating composition on the colored coating film (S22)

[0198] The two-component coating composition is applied to the colored coating film by the same method as in the first embodiment. The two-component coating composition may be applied to an uncured colored coating film or a cured colored coating film.

[0199] (III) Step of pressing the coated surface (S23)

[0200] The coated surface of the object to be coated is pressed while being heated in the same manner as in the first embodiment, thereby curing the two-component coating composition to obtain a second coating film.

[0201] The first and second coating films formed by the two-component coating composition have excellent weather resistance, design and water resistance. Therefore, the obtained coated articles are suitable for, for example, exterior decoration of automobiles and architectural uses. In particular, the obtained coated articles are suitable for automobile parts such as spoilers, pillars, bumpers, mirror covers, grilles, door handles, etc.

[0202] Example

[0203] The present invention will be described in more detail by the following examples, but the present invention is not limited thereto. In the examples, "parts" and "%" are based on mass standards unless otherwise specified.

[0204] [Example 1]

[0205] (1) Preparation of two-component coating composition

[0206] 100 parts of polyol (SANNIX GP-250, manufactured by Sanyo Chemical Industries, Ltd., hydroxyl value of 670 mgKOH / g, average number of hydroxyl groups of 3), UVA (Tinuvin 384-2, manufactured by BASF, benzotriazole compound), UVA (Tinuvin 400, manufactured by BASF, triazine compound), HALS (HOSTAVIN 3058, manufactured by Clariant Chemicals, molecular weight 449, N-CO-R type), 0.3 parts of curing catalyst (K-KAT XK-640, manufactured by Kusumoto Chemicals, Bi-containing organic metal catalyst) (effective ingredient amount) were mixed to prepare the main agent. In the table, the amount of each UVA and HALS is described as a ratio (PHR: mass %) relative to 100 mass % of the resin solid content (polyol and curing agent).

[0207] Separately, as a curing agent, 218 parts of an isocyanurate compound (Desmodur N3600, manufactured by Sumika Covestro Urethane Co., Ltd., urate form of HDI) was prepared.

[0208] NCO / OH=1.0 / 1.0, and the solvent content of the two-component coating composition is 0%.

[0209] (2) Production of painted items

[0210] As the object to be coated, a CFRP plate (epoxy resin) was prepared. A masking tape (thickness 100 μm) was pasted on the object to be coated as a spacer. The main agent and curing agent of the obtained two-component coating composition were mixed. The two-component coating composition was applied to the object to be coated by a scraper method. Then, a pressing member heated to 80° C. was used to press the coated surface for 5 minutes to obtain a first coating film having a film thickness (100 μm) suitable for the above-mentioned spacer. In this way, a coated article was obtained.

[0211] [Examples 2 to 16 and Comparative Examples 1 to 12]

[0212] (1) Preparation of two-component coating composition

[0213] Except for changing the type and amount of each component as described in Tables 1 to 3, the main agent and the curing agent were prepared by the same procedure as in Example 1.

[0214] It should be noted that ethyl acetate was mixed into the main agent as an organic solvent in Examples 10 to 12 and Comparative Examples 7 to 10. In Tables 1 to 3, the amount of solvent is described as a ratio relative to the two-component coating composition.

[0215] (2) Production of painted items

[0216] Using the two-component coating compositions obtained in Examples 2 to 15 and Comparative Examples 1 to 7, 11, and 12, the same operation as in Example 1 was carried out to obtain coated articles.

[0217] The two-component coating compositions obtained in Comparative Examples 8 to 10 were electrostatically coated on CFRP plates using a Cartridge Bell (manufactured by ABB, rotary atomizing coater) to obtain coated articles. The thickness of the first coating film is shown in Tables 1 to 3.

[0218] In Example 16, a coated article was obtained in the same manner as in Example 1 except that a CFRP plate having a primer film (thickness 20 μm) was used as the coated object. The primer film was formed by electrostatically coating a primer containing a coloring pigment using a Cartridge Bell (manufactured by ABB, rotary atomizer).

[0219] The ingredients in the table above are as follows.

[0220] (Polyhydroxy compounds)

[0221] SANNIX GP-400: manufactured by Sanyo Chemical Industries, Ltd., polyether polyol, hydroxyl value 400 mgKOH / g, average hydroxyl number 3;

[0222] SANNIX GP-600: manufactured by Sanyo Chemical Industries, Ltd., polyether polyol, hydroxyl value 280 mgKOH / g, average hydroxyl number 3;

[0223] SANNIX GP-1000: manufactured by Sanyo Chemical Industries, Ltd., polyether polyol, hydroxyl value 160 mgKOH / g, average hydroxyl number 3;

[0224] Desmophen VPLS2249 / 1: manufactured by Sumika Covestro Urethane Co., Ltd., polyester polyol, hydroxyl value of 512 mgKOH / g, average hydroxyl number of 3 or more;

[0225] Desmophen XP2488: manufactured by Sumika Covestro Urethane Co., Ltd., polyester polyol, hydroxyl value of 528 mgKOH / g, average hydroxyl number of 3 or more;

[0226] SANNIX PP-200: manufactured by Sanyo Chemical Industries, Ltd., polyether polyol, hydroxyl value 560 mgKOH / g, average hydroxyl number 2;

[0227] SANNIX PP-600: manufactured by Sanyo Chemical Industries, Ltd., polyether polyol, hydroxyl value: 187 mgKOH / g, average number of hydroxyl groups: 2.

[0228] (Curing Catalyst)

[0229] TVS TIN LAU: Sn-containing organometallic catalyst manufactured by Nitto Kasei Co., Ltd.

[0230] (Curing agent)

[0231] Duranate 24A-100: manufactured by Asahi Kasei Corporation, biuret form of HDI;

[0232] Desmodur N3400: manufactured by Sumika Covestro Urethane Co., Ltd., a dimer of HDI.

[0233] The following evaluations were performed using the two-component coating compositions prepared in Examples and Comparative Examples and the coated articles. The evaluation results are shown in Tables 1 to 3.

[0234] (1) Workability

[0235] A curing agent was added to the prepared main agent. After adding the curing agent, the mixture was mixed for 15 seconds and the sample was taken out. The time when the sample was taken out was set as the time when the coating operation started: 0 seconds, and the sample was stirred with a spatula. The fluidity disappeared due to the curing reaction of the main agent and the curing agent, and the time required to reach a state where the sample did not fall immediately was measured as the coating operation time, and evaluated according to the following standards.

[0236] (Evaluation Criteria)

[0237] Good: coating operation time is more than 60 seconds and less than 600 seconds;

[0238] Yes: The coating operation time is 30 seconds or more and less than 60 seconds, or 600 seconds or more and less than 900 seconds;

[0239] Bad: Coating operation time is less than 30 seconds or more than 900 seconds.

[0240] (2) Edge collapse (sagging) of uncured coating film

[0241] (2-1) Film formation by open pressure coating

[0242] A curing agent was added to the prepared main agent. After the curing agent was added, the mixture was mixed with a spatula for 15 seconds. The obtained coating composition was applied to an ABS plate with a spatula (film thickness: 100 μm).

[0243] (2-2) Coating by spraying

[0244] A curing agent was added to the prepared main agent. After the curing agent was added, the mixture was mixed with a spatula for 15 seconds. The obtained coating composition was applied to an ABS plate by air spraying (film thickness: 100 μm).

[0245] (2-3) Evaluation of coating film flowability

[0246] The coated ABS plates obtained in (2-1) and (2-2) were left to stand at 23°C for 10 minutes and then stood vertically. After 5 minutes, it was observed whether the coating material flowed onto the ground surface or not, and the evaluation was performed according to the following criteria.

[0247] (Evaluation Criteria)

[0248] Good: The paint does not flow to the ground surface;

[0249] Bad: Paint is dripping onto ground surface.

[0250] (3) Weather resistance

[0251] The coated articles were subjected to an accelerated weathering test for 800 hours in accordance with JIS B 7753 using Sunshine Weather Meter S80 (Sunshine carbon arc accelerated weathering tester, manufactured by Suga Testing Machine Co., Ltd.). The 60° gloss value of the coating before and after the test was measured using a gloss meter GN-268Plus (manufactured by KONICA MINOLTA Co., Ltd.), and the gloss retention was calculated using the following formula. The calculated gloss retention was evaluated according to the following criteria.

[0252] Gloss retention rate = 100 × {(60° gloss value before the test) - (60° gloss value after the test)} / (60° gloss value before the test)

[0253] (Evaluation Criteria)

[0254] Good: gloss retention rate is above 80%;

[0255] Yes: gloss retention rate is above 60% and less than 80%;

[0256] Poor: Gloss retention is less than 60%.

[0257] (4) Water resistance

[0258] The test plate obtained by the same operation as above was immersed in a water tank stored at 40°C for 240 hours. After that, the test plate was lifted from the water and dried at room temperature for 1 hour. Then, 10 cuts were made vertically and horizontally at intervals of 1 mm on the coating of the test plate with a cutter, and Cellotape (registered trademark) (manufactured by NICHIBAN) was pasted on it and then peeled off. The number of grids with residual coating in 100 grids was counted. The more grids with residual coating, the better the adhesion after the water resistance test and the higher the water resistance. The number of counted grids was evaluated according to the following standards.

[0259] (Evaluation Criteria)

[0260] Good: The number of counted grids is 81 or more;

[0261] Yes: The number of grids counted is more than 60 and less than 80;

[0262] Bad: The number of grids counted is 59 or less.

[0263]

[0264]

[0265]

[0266] Industrial Applicability

[0267] The two-component coating composition of the present invention can be applied to coating methods other than conventional spray coating, such as open pressure coating. The two-component coating composition of the present invention can produce a coating film having excellent weather resistance and water resistance, and is therefore particularly suitable for exterior decoration.

[0268] This application claims priority based on Japanese Patent Application No. 2020-180762 filed in Japan on October 28, 2020, the entire contents of which are incorporated herein by reference.

[0269] Explanation of symbols

[0270] 100A, 100B, 200: painted articles;

[0271] 10: Object to be coated;

[0272] 20A: 1st coating;

[0273] 20B: 2nd coating film;

[0274] 30: Other coatings;

[0275] 31: Primer coating;

[0276] 32: Transparent coating;

[0277] 40: Colored coating.

Claims

1. A two-component coating composition comprising a main agent and a curing agent, The main agent comprises a polyhydroxy compound, a curing catalyst and an ultraviolet absorber. The curing agent comprises an isocyanurate compound, The hydroxyl value of the polyhydroxy compound is 500 mgKOH / g or more and 1000 mgKOH / g or less, The average number of hydroxyl groups in the polyhydroxy compound is 3 or more. The content of the curing catalyst is 0.05 parts by mass or more and 3 parts by mass or less relative to 100 parts by mass of the polyhydroxy compound. The content of the solvent is 10% by mass or less, It is used for exterior decoration and for open pressure coating.

2. The two-component coating composition according to claim 1, wherein The isocyanurate compound includes a trimer of hexamethylene diisocyanate.

3. The two-component coating composition according to claim 1 or 2, wherein: The above main agent further comprises a light stabilizer.

4. The two-component coating composition according to claim 1 or 2, wherein: The polyhydroxy compound is at least one selected from the group consisting of polyester polyol, polyether polyol and polycarbonate polyol.

5. The two-component coating composition according to claim 1 or 2, wherein: The ratio of the isocyanate group equivalent of the isocyanurate compound to the hydroxyl group equivalent of the polyol compound: NCO / OH is 0.5 / 1 or more and 2 / 1 or less.

6. The two-component coating composition according to claim 1 or 2, wherein: The curing catalyst includes at least one organic metal catalyst, and the organic metal catalyst includes a metal element selected from the group consisting of Bi, Zn, Al, Zr and Sn.

7. A method for producing a coated article, comprising the following steps: The process of preparing the object to be coated; A step of applying the two-component coating composition according to any one of claims 1 to 6 to the object to be coated; and A step of pressing the surface of the object to be coated on which the two-component coating composition is applied while heating to cure the two-component coating composition to form a first coating film.

8. The method for producing a coated article according to claim 7, wherein: The thickness of the first coating film is 80 μm or more.

9. A method for producing a coated article, comprising the following steps: The process of preparing an object to be coated with a colored coating film; A step of applying the two-component coating composition according to any one of claims 1 to 6 onto the colored coating film; and A step of pressing the surface of the object to be coated with the two-component coating composition while heating to cure the two-component coating composition to form a second coating film.

10. The method for producing a coated article according to claim 9, wherein: The second coating film has a thickness of 80 μm or more.

Citation Information

Patent Citations

  • Dispersion board, chlorination furnace, and production method of metal chloride

    JP2020180762A

  • Die for forming in-mold coated article and method for manufacturing in-mold coated article

    WO2010113847A1

  • Coating composition and coating film forming method

    JP2017193705A