A method for preparing graphite for lithium battery by using silver salt catalyzed coke at low temperature

The preparation of graphite for lithium batteries by catalyzing coke at low temperature by silver salt, solved the problem of high temperature and high energy consumption and insufficient graphitization in the preparation process of artificial graphite of lithium-ion battery negative electrode materials, and achieved efficient and safe low temperature preparation, with excellent electrochemical properties and Recyclable process.

CN116395684BActive Publication Date: 2024-11-22WUXI HUARUI XINNENG BATTERY MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310483320.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-22
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

There are problems of high temperature and high energy consumption and safety hazards in the preparation process of artificial graphite, an existing lithium-ion battery negative electrode material, and the degree of graphitization at low temperature is not enough to meet the performance requirements of lithium batteries.

Method used

The graphite for lithium batteries is prepared by using silver salt catalytic coke at low temperature. Through the steps of soaking in ethanol solution, dispersing silver salt, ammonia water reaction and calcining, small nanoparticles are formed to achieve graphitization, and then the nitric acid solution removes impurities to obtain a high degree of graphitization. graphite for lithium batteries.

Benefits of technology

It has achieved efficient preparation of lithium battery-grade artificial graphite at low temperatures, with a degree of graphitization of more than 90%, with high specific capacity, excellent rate performance and good cycle stability, simple process, suitable for large-scale production, and recycling silver salt.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004221938140000011
    Figure HDA0004221938140000011
  • Figure HDA0004221938140000012
    Figure HDA0004221938140000012
  • Figure HDA0004221938140000021
    Figure HDA0004221938140000021
Patent Text Reader

Abstract

The present invention provides a method for preparing lithium-powered graphite by using silver salt-catalyzed coke at low temperature, comprising the following steps: (1) soaking the coke in an ethanol solution, and then performing solid-liquid separation to obtain product A; (2) dispersing the silver salt in an ethylene glycol solution, adding product A, reacting the obtained mixture at a first preset temperature for a first preset time, adding ammonia water, reacting at a second preset temperature for a second preset time, and performing solid-liquid separation to obtain product B; (3) calcining product B in an inert atmosphere at 600-1200°C for 4-10h, and then soaking the product in a nitric acid solution, and performing solid-liquid separation to obtain graphite material for lithium-powered graphite. The present invention can realize the low-temperature preparation of graphite material, and the prepared artificial graphite has a graphitization degree of more than 90%, and exhibits high specific capacity, excellent rate performance and good cycle stability when used as a negative electrode material for lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of negative electrode materials for lithium ion batteries, and in particular to a method for preparing graphite for lithium batteries under low temperature by using silver salt-catalyzed coke. Background Art

[0002] With the policy development requirements of "carbon neutrality" and "carbon peak", fuel vehicles will gradually be replaced by new energy vehicles. Among the new energy vehicles currently on the market, lithium-ion driven ones account for nine-tenths of the market share. In lithium-ion batteries, graphite is the negative electrode material. In 2022, the amount of graphite used in the lithium-ion vehicle market will be 720,000 tons. The rate performance of artificial graphite is better than that of natural graphite, so artificial graphite accounts for two-thirds of its share. Commercial artificial graphite uses thermoinduced phase change technology to transform soft carbon into artificial graphite at temperatures above 2800°C, such as CN101648808B and US20020012845A1. The high temperature process of 2800°C is a high energy consumption process, and the production process is full of dangers, so it is of great significance to reduce the preparation temperature of artificial graphite.

[0003] CN108101043B uses magnesium metal as a catalyst to obtain artificial graphite with a graphitization degree higher than 90% at low temperature. Although its graphitization degree can meet the performance requirements of lithium battery negative electrode graphite, its preparation process is still full of dangers. Because commercial artificial graphite needs to be prepared in tons, a large amount of magnesium catalyst is required. Magnesium will release a lot of heat during the high-temperature catalytic process, and the huge heat released by a large amount of magnesium will become a hidden danger in production safety. However, some researchers have prepared artificial graphite under low temperature and mild conditions (Carbon 75 (2014) 95-103), but its graphitization degree is less than 50%, which cannot meet the performance requirements of lithium battery negative electrode graphite and be used. Therefore, it is necessary to develop a mild low-temperature preparation technology for artificial graphite, and its product can meet the performance requirements of lithium battery negative electrode materials. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for preparing lithium battery graphite at low temperature by using silver salt to catalyze coke, and its performance can meet the standard requirements of lithium battery graphite. The lithium battery graphite prepared by the method of the present invention has high cycle specific capacity, good rate performance, and good cycle stability.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing graphite for lithium battery at low temperature by using silver salt to catalyze coke, comprising the following steps:

[0007] (1) soaking the coke in an ethanol solution, and then performing solid-liquid separation to obtain product A;

[0008] (2) dispersing the silver salt into an ethylene glycol solution, adding product A, reacting the obtained mixture at a first preset temperature for a first preset time, adding aqueous ammonia, reacting at a second preset temperature for a second preset time, and performing solid-liquid separation to obtain product B;

[0009] (3) calcining product B at 600-1200° C. in an inert atmosphere for 4-10 hours, then soaking it in a nitric acid solution, and performing solid-liquid separation to obtain a graphite material for lithium battery.

[0010] Preferably, step (1) specifically comprises: soaking the coke in an ethanol solution, stirring under heating conditions, filtering, and drying to obtain product A.

[0011] Preferably, in step (1), the coke is coal-derived coke or petroleum-derived coke.

[0012] Preferably, in step (1), the ratio of coke to ethanol solution is (1-100) g: (5-500) ml.

[0013] Preferably, in step (2), the first preset temperature is 150° C., the first preset time is 5 hours, the second preset temperature is 180° C., and the second preset time is 3 hours.

[0014] Preferably, in step (2), the silver salt is silver iodide, silver acetate, silver phosphate, silver perchlorate or silver salicylate.

[0015] Preferably, in step (2), the ratio of silver salt to product A is (1-6) ml: (1-100) g.

[0016] Preferably, in step (2), the concentration of ammonia water is 2 wt %, and the ratio of silver salt to ammonia water is (1-6) ml: (1-10) ml.

[0017] Preferably, in step (2), the ratio of silver salt to ethylene glycol solution is (1-6) ml: (2-50) ml.

[0018] Preferably, in step (3), the inert atmosphere is a nitrogen atmosphere.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The coke used in the present invention belongs to a soft carbon material. When the coke is soaked in an ethanol solution, the non-layered structure can be effectively removed, so that the resistance is reduced when the coke is thermodynamically regularized during the subsequent calcination process; the silver salt forms an atomic-level complex with ethylene glycol, which can be effectively diffused in the coke, and then forms dispersed nanoparticles under the action of ammonia water. These uniformly distributed silver nanoparticles have a large number of dangling bonds, so they have high catalytic activity and can effectively catalyze the graphitization of the coke during the subsequent calcination process to obtain lithium-grade artificial graphite. Therefore, the present invention can realize the low-temperature preparation of graphite materials, and the process is simple, the repeatability is good, and it can be mass-produced, and the silver salt obtained by impurity removal can be effectively recycled for secondary use; the degree of graphitization of the artificial graphite prepared by the method is greater than 90%, and when it is used as a negative electrode material for lithium-ion batteries, it exhibits excellent electrochemical properties such as high specific capacity, excellent rate performance and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is the X-ray diffraction spectrum of the lithium-grade artificial graphite prepared in Examples 1 to 4 of the present invention.

[0022] Figure 2 This is a scanning electron microscope image of the lithium-grade artificial graphite prepared in Example 2 of the present invention.

[0023] Figure 3 This is the Raman spectrum of the lithium-grade artificial graphite prepared in Example 3 of the present invention.

[0024] Figure 4 This is a cycle stability diagram of the lithium-grade artificial graphite prepared in Example 4 of the present invention as a lithium-ion negative electrode material. DETAILED DESCRIPTION

[0025] In order to further understand the present invention, the present invention is described below in conjunction with embodiments. These descriptions are only to further explain the features and advantages of the present invention and are not intended to limit the claims of the present invention.

[0026] The method for preparing graphite for lithium battery at low temperature by silver salt catalyzed coke of the present invention comprises the following steps:

[0027] (1) soaking the coke in an ethanol solution, stirring under heating conditions, filtering and drying to obtain product A;

[0028] (2) Dispersing the silver salt in an ethylene glycol solution, stirring, then adding product A, stirring the resulting mixture at 150° C. for 5 h, then slowly adding ammonia water, and stirring at 180° C. for 3 h; filtering and drying the product to obtain product B;

[0029] (3) calcining product B at 600-1200° C. in a nitrogen atmosphere for 4-10 h, and soaking the product in a 0.1 M nitric acid solution to remove silver impurities, thereby obtaining a graphite material for lithium batteries with a graphitization degree greater than 90%.

[0030] In the step (1), the coke is either coal-derived coke or petroleum-derived coke.

[0031] In the step (1), the ratio of coke to ethanol solution is (1-100) g: (5-500) ml, the heating temperature is preferably 80° C., and the stirring time is preferably 5 h.

[0032] In the step (2), the silver salt is any one of silver iodide, silver acetate, silver phosphate, silver perchlorate or silver salicylate.

[0033] In the step (2), the ratio of silver salt to ethylene glycol solution is (1-6) g: (2-50) ml; the concentration of ammonia water is preferably 2 wt%, and the ratio of silver salt to ammonia water is (1-6) g: (1-10) ml; the ratio of silver salt to product A is (1-6) g: (1-100) g.

[0034] Example 1

[0035] (1) 1 g of coal-derived coke was soaked in 5 ml of 50 wt% ethanol solution, stirred at 80° C. for 5 h, filtered and dried to obtain product A;

[0036] (2) Disperse 1 g of silver iodide in 2 ml of ethylene glycol solution, stir for 3 h, then add 1 g of product A, stir the resulting mixture at 150° C. for 5 h, then slowly add 1 ml of 2 wt % ammonia water, and continue stirring at 180° C. for 3 h; filter and dry the product to obtain product B;

[0037] (3) Calcine product B at 600° C. in a nitrogen atmosphere for 10 h, soak the product in a 0.1 M nitric acid solution to remove silver impurities, and obtain a graphite material for lithium batteries.

[0038] Example 2

[0039] (1) 40 g of petroleum-derived coke was soaked in 100 ml of a 50 wt% ethanol solution, stirred at 80° C. for 5 h, filtered and dried to obtain product A;

[0040] (2) 2 g of silver acetate was dispersed in 10 ml of ethylene glycol solution, and after stirring for 3 h, 10 g of product A was added, and the obtained mixture was continuously stirred at 150° C. for 5 h, and then 3 ml of 2 wt % ammonia water was slowly added, and the mixture was continuously stirred at 180° C. for 3 h; the product was filtered and dried to obtain product B;

[0041] (3) Calcine product B at 800° C. in a nitrogen atmosphere for 8 h, soak the product in a 0.1 M nitric acid solution to remove silver impurities, and obtain graphite material for lithium batteries.

[0042] Example 3

[0043] (1) 80 g of petroleum-derived coke was soaked in 300 ml of a 50 wt% ethanol solution, stirred at 80° C. for 5 h, filtered and dried to obtain product A;

[0044] (2) 5 g of silver perchlorate was dispersed in 30 ml of ethylene glycol solution, and after stirring for 3 h, 80 g of product A was added, and the obtained mixture was continuously stirred at 150° C. for 5 h, and then 8 ml of 2 wt % ammonia water was slowly added, and the mixture was continuously stirred at 180° C. for 3 h; the product was filtered and dried to obtain product B;

[0045] (3) Calcine product B at 1000° C. in a nitrogen atmosphere for 6 h, soak the product in a 0.1 M nitric acid solution to remove silver impurities, and obtain graphite material for lithium batteries.

[0046] Example 4

[0047] (1) 100 g of coal-derived coke was soaked in 500 ml of a 50 wt% ethanol solution, stirred at 80° C. for 5 h, filtered and dried to obtain product A;

[0048] (2) 6 g of silver salicylate was dispersed in 50 ml of ethylene glycol solution, and after stirring for 3 h, 100 g of product A was added, and the mixture was stirred at 150° C. for 5 h, and then 10 ml of 2 wt % ammonia water was slowly added, and the mixture was stirred at 180° C. for 3 h; the product was filtered and dried to obtain product B;

[0049] (3) Calcine product B at 1200° C. in a nitrogen atmosphere for 4 h, soak the product in a 0.1 M nitric acid solution to remove silver impurities, and obtain a graphite material for lithium batteries.

[0050] See attached figure, Figure 1 This is the X-ray diffraction spectrum of the lithium-grade artificial graphite prepared in Examples 1 to 4 of the present invention. The horizontal axis is the angle; the vertical axis is the relative intensity, and 30wt% of single silicon is used as a reference standard. It can be seen from the figure that graphite material is obtained, and the highest peak corresponds to the (002) diffraction plane of graphite. After calculation by the formula, it is obtained that the degree of graphitization is 92%.

[0051] Figure 2 This is a scanning electron microscope image of the lithium-grade artificial graphite prepared in Example 2 of the present invention. It can be seen from the image that large flake artificial graphite is obtained.

[0052] Figure 3This is the Raman spectrum of the lithium-grade artificial graphite prepared in Example 3 of the present invention. The intensity of the ordered G peak is much higher than the intensity of the disordered D peak, indicating that the product has a high degree of graphitization.

[0053] Figure 4 This is a cycle stability diagram of the lithium-grade artificial graphite prepared in Example 4 of the present invention as a negative electrode material for lithium-ion batteries. It can be seen from the figure that after 600 cycles, the specific capacity has not decayed, thus proving that the obtained low-temperature artificial graphite has good electrochemical performance as a negative electrode for lithium batteries.

[0054] The present invention is not limited to the specific embodiments listed above. Those skilled in the art can make various equivalent modifications, equivalent replacements, component additions and subtractions, and recombinations based on the working principle of the present invention and the specific embodiments given above, so as to form more new embodiments.

Claims

1. A method for preparing graphite for lithium battery at low temperature by using silver salt catalyzed coke, characterized in that: The steps include: (1) soaking the coke in an ethanol solution, and then performing solid-liquid separation to obtain product A; the ratio of coke to ethanol solution is (1-100) g: (5-500) ml; (2) dispersing the silver salt into an ethylene glycol solution, adding product A, reacting the obtained mixture at a first preset temperature for a first preset time, adding aqueous ammonia, reacting at a second preset temperature for a second preset time, and performing solid-liquid separation to obtain product B; (3) calcining product B at 600-1200°C in an inert atmosphere for 4-10 hours, then soaking it in a nitric acid solution, and performing solid-liquid separation to obtain a graphite material for lithium battery; Step (1) specifically comprises: soaking the coke in an ethanol solution, stirring under heating conditions, filtering, and drying to obtain product A.

2. The method for preparing graphite for lithium battery at low temperature using silver salt catalyzed coke according to claim 1, characterized in that: In step (1), the coke is coal-derived coke or petroleum-derived coke.

3. The method for preparing graphite for lithium battery at low temperature using silver salt catalyzed coke according to claim 1, characterized in that: In step (2), the first preset temperature is 150° C., the first preset time is 5 hours, the second preset temperature is 180° C., and the second preset time is 3 hours.

4. The method for preparing graphite for lithium battery at low temperature using silver salt catalyzed coke according to claim 1, characterized in that: In step (2), the silver salt is silver iodide, silver acetate, silver phosphate, silver perchlorate or silver salicylate.

5. The method for preparing graphite for lithium battery at low temperature using silver salt catalyzed coke according to claim 1, characterized in that: In step (2), the ratio of silver salt to product A is (1-6) ml: (1-100) g.

6. The method for preparing graphite for lithium battery at low temperature by using silver salt catalyzed coke according to claim 1, characterized in that: In step (2), the concentration of ammonia water is 2 wt %, and the ratio of silver salt to ammonia water is (1-6) ml: (1-10) ml.

7. The method for preparing graphite for lithium battery at low temperature by using silver salt catalyzed coke according to claim 1, characterized in that: In step (2), the ratio of silver salt to ethylene glycol solution is (1-6) ml: (2-50) ml.

8. The method for preparing graphite for lithium battery at low temperature by using silver salt catalyzed coke according to claim 1, characterized in that: In step (3), the inert atmosphere is a nitrogen atmosphere.

Citation Information

Patent Citations

  • Preparation method of graphite material

    CN101648808B

  • Preparation method and application of coal-derived artificial graphite material

    CN108101043B

  • Negative active material for rechargeable lithium battery and method of preparing the same

    US20020012845A1

  • Carbon material for using as catalyst carrier

    CN105073260A

  • Preparation method for high-strength high-density isotropic impregnation silver carbon / graphite composite material

    CN105215331A