A polymerizable deep eutectic gel and its preparation method and application
By blending lignin in rice husk with a polymerizable deep eutectic solvent and performing photoinitiated polymerization, a polymerizable deep eutectic gel with high mechanical strength and electrical conductivity was prepared, which solved the problem of traditional flexible sensor material mechanical properties and The problem of insufficient conductivity is solved, and the effect of high sensitivity and multiple recycling is achieved.
Patent Information
- Application Number
- CN202310377935.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-04-11
AI Technical Summary
Traditional flexible sensor materials have deficiencies in mechanical properties and electrical conductivity, making it difficult to combine high strength and high sensitivity. Phase separation is prone to occur during the stretching process, resulting in low sensing sensitivity.
By blending lignin from rice husk with a polymerizable deep eutectic solvent to form dense hydrogen bonds in the polymer network, and using a photoinitiator for UV polymerization, a polymer with high mechanical strength, electrical conductivity, and sensitivity was prepared. of polymerizable deep eutectic gels.
The prepared gel has excellent mechanical strength and toughness, with a tensile strength as high as 1210.9KPa and an elongation at break as high as 1445.8%. It also has high sensitivity, high conductivity and stability, and is suitable for multiple recycling of flexible sensor materials. .
Smart Images

Figure CN116396448B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sensor technology, and specifically provides a polymerizable deep eutectic gel and a preparation method and application thereof. Background Art
[0002] The statements herein merely provide background information related to the present disclosure and do not necessarily constitute prior art.
[0003] Traditional electronic strain sensors are mostly based on metal and semiconductor materials, which have poor portability, flexibility and wearability. Flexible and stretchable strain sensors are gaining more and more attention due to their excellent performance and comfort. Organisms contain countless sensors that convert external stimuli into bioelectric signals and transmit them to neurons and the brain, inspiring more and more researchers to study flexible sensors.
[0004] The application of gel materials formed based on polymerizable deep eutectic solvents in flexible sensors has been reported. For example, the prior art discloses a polyacrylamide hydrogel using in-situ polymerization of hyperbranched polyester, using this hydrogel as a shell, filling a deep eutectic solvent, and initiating polymerization of the deep eutectic solvent filled in the hydrogel by ultraviolet light to obtain a composite material. However, this type of material still has weak mechanical properties in practical applications, is prone to phase separation during stretching, and has weak conductivity and low sensing sensitivity. Therefore, research on the preparation of high-strength and tough conductive hydrogels, exploring the relationship between their structure and performance, and improving conductivity and sensing sensitivity at the same time are still urgent issues to be solved. Summary of the invention
[0005] In view of the problem that flexible sensor materials in the prior art are difficult to have both high strength and high sensitivity, the present invention provides a polymerizable deep eutectic gel, which is formed by blending a polymerizable deep eutectic solvent with a macromolecular organic polymer lignin in rice husk to form dense hydrogen bonds in the polymer network, and then using a photoinitiator to perform ultraviolet light polymerization. The gel has excellent mechanical strength and toughness, as well as high sensitivity, high conductivity, high adhesion and stability, and can be used as a flexible sensor material for multiple cycles.
[0006] The first aspect of the present invention provides a method for preparing a polymerizable deep eutectic gel, and the specific steps include: adding rice husks into a polymerizable deep eutectic solvent, heating and stirring to extract lignin in the rice husks; then extracting the supernatant by centrifugation, adding a photoinitiator to the supernatant, and performing photopolymerization under ultraviolet light to obtain a polymerizable deep eutectic gel.
[0007] The second aspect of the present invention provides a polymerizable deep eutectic gel obtained by the above-mentioned preparation method.
[0008] A third aspect of the present invention provides a use of the above-mentioned polymerizable deep eutectic gel in a flexible sensor.
[0009] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:
[0010] 1. The present invention utilizes a simple method to extract lignin from biomass rice husk materials, and blends a polymerizable deep eutectic solvent with the macromolecular organic polymer lignin in the rice husk to form dense hydrogen bonds in the polymer network, and then adds a photoinitiator to initiate polymerization under ultraviolet light, thereby preparing a polymerizable deep eutectic gel, which effectively improves the mechanical properties of the hydrogel.
[0011] 2. Compared with traditional biomass sensor gels, the polymerizable deep eutectic gel prepared by the method of the present invention has excellent mechanical strength and toughness, with a tensile strength of up to 1210.9 KPa and an elongation at break of up to 1445.8%. In addition, the gel also has high sensitivity, high conductivity, high adhesion and stability, and can be used as a flexible sensor material for multiple cycles.
[0012] 3. The preparation method of the polymerizable deep eutectic gel provided by the present invention is simple, novel, green, low-energy consumption and low-cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0014] Figure 1 The present invention provides a flow chart for preparing the polymerizable deep eutectic gel;
[0015] Figure 2 This is a graph showing the relative current variation when the polymerizable deep eutectic gel prepared in Example 3 detects different bending angles of the finger based on a flexible sensor;
[0016] Figure 3 is a graph showing the relative current variation when the polymerizable deep eutectic gel prepared in Example 3 detects different wrist bending angles based on a flexible sensor;
[0017] Figure 4 This is a graph showing the relative current changes when the polymerizable deep eutectic gel prepared in Example 3 detects different knee bending angles based on a flexible sensor. DETAILED DESCRIPTION
[0018] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0019] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0020] In view of the problem that flexible sensor materials in the prior art are difficult to have both high strength and high sensitivity, the present invention provides a polymerizable deep eutectic gel and a preparation method and application thereof.
[0021] A typical embodiment of the present invention provides a method for preparing a polymerizable deep eutectic gel, and the specific steps include: adding rice husks into a polymerizable deep eutectic solvent, heating and stirring to extract lignin in the rice husks; then extracting the supernatant by centrifugation, adding a photoinitiator to the supernatant, and performing photopolymerization under ultraviolet light to obtain a polymerizable deep eutectic gel.
[0022] Principle of this experiment: The present invention uses a simple method to extract the macromolecular organic polymer lignin from the biomass rice husk material into a deep eutectic solvent, and then blends the polymerizable deep eutectic solvent and lignin to form dense hydrogen bonds in the polymer network. Then, the present invention adds a photoinitiator, which is a type of compound that can absorb energy of a certain wavelength in the ultraviolet light region (250-420nm) or the visible light region (400-800nm) to generate free radicals, cations, etc., thereby initiating monomer polymerization, cross-linking and curing. It can initiate the polymerization of monomers in the deep eutectic solvent, thereby generating an elastomer and obtaining a gel.
[0023] In some embodiments, choline chloride and acrylic acid solution are mixed, heated and stirred until the solution becomes transparent to obtain a polymerizable deep eutectic solvent.
[0024] In some embodiments, the molar ratio of choline chloride to acrylic acid solution is 1:2.
[0025] In some embodiments, the concentration of the acrylic acid solution is 98%; the concentration of the choline chloride solution is 98%.
[0026] In some embodiments, the heating and stirring time after mixing the choline chloride and acrylic acid solution is 3-4 hours, and the temperature is 90-95°C.
[0027] In some embodiments, the mass volume ratio of rice husk to polymerizable deep eutectic solvent is 1 g:20 ml.
[0028] In order to better extract the macromolecular organic polymer lignin from the rice husk, it is necessary to fully stir it at high temperature. In some embodiments, after the rice husk is added to the polymerizable deep eutectic solvent, the heating and stirring time is 10-120 minutes at a temperature of 90-100°C.
[0029] In some embodiments, the mass volume ratio of the photoinitiator to the supernatant is 4 g:12675 ml.
[0030] In some embodiments, the photoinitiator is 2959 and its concentration is 99%.
[0031] In some embodiments, after adding the photoinitiator to the supernatant, the mixture is stirred for 5-10 minutes in a light-proof condition before photopolymerization.
[0032] Another embodiment of the present invention provides a polymerizable deep eutectic gel obtained by the above preparation method.
[0033] A third embodiment of the present invention provides an application of the above-mentioned polymerizable deep eutectic gel in a flexible sensor.
[0034] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0035] Example 1
[0036] This embodiment provides a method for preparing a polymerizable deep eutectic gel, which comprises the following steps:
[0037] (1) 25 g of choline chloride and 25.7 g of acrylic acid solution were mixed, heated and stirred at 90° C. for 3 h until the solution became transparent, to obtain a polymerizable deep eutectic solvent;
[0038] (2) adding 2 g of rice husk into 40 ml of a polymerizable deep eutectic solvent and heating and stirring at 100 °C for 10 min to extract lignin from the rice husk;
[0039] (3) centrifuging the solution obtained in step (2) and extracting the supernatant;
[0040] (4) adding photoinitiator 2959 to the supernatant obtained in step (3), wherein the mass volume ratio of photoinitiator 2959 to supernatant is 4:12675, and stirring for 5 minutes in a dark environment;
[0041] (5) The solution obtained in step (4) is subjected to photopolymerization under ultraviolet light to prepare a polymerizable deep eutectic gel.
[0042] Example 2
[0043] This embodiment provides a method for preparing a polymerizable deep eutectic gel, which comprises the following steps:
[0044] (1) 25 g of choline chloride and 25.7 g of acrylic acid solution were mixed, heated and stirred at 90° C. for 3 h until the solution became transparent, to obtain a polymerizable deep eutectic solvent;
[0045] (2) adding 2 g of rice husk into 40 ml of a polymerizable deep eutectic solvent and heating and stirring at 100 °C for 30 min to extract lignin from the rice husk;
[0046] (3) centrifuging the solution obtained in step (2) and extracting the supernatant;
[0047] (4) adding photoinitiator 2959 to the supernatant obtained in step (3), wherein the mass volume ratio of photoinitiator 2959 to supernatant is 4:12675, and stirring for 5 minutes in a dark environment;
[0048] (5) The solution obtained in step (4) is subjected to photopolymerization under ultraviolet light to prepare a polymerizable deep eutectic gel.
[0049] Example 3
[0050] This embodiment provides a method for preparing a polymerizable deep eutectic gel, which comprises the following steps:
[0051] (1) 25 g of choline chloride and 25.7 g of acrylic acid solution were mixed, heated and stirred at 90° C. for 3 h until the solution became transparent, to obtain a polymerizable deep eutectic solvent;
[0052] (2) adding 2 g of rice husk into 40 ml of a polymerizable deep eutectic solvent and heating and stirring at 100 °C for 60 min to extract lignin from the rice husk;
[0053] (3) centrifuging the solution obtained in step (2) and extracting the supernatant;
[0054] (4) adding photoinitiator 2959 to the supernatant obtained in step (3), wherein the mass volume ratio of photoinitiator 2959 to supernatant is 4:12675, and stirring for 5 minutes in a dark environment;
[0055] (5) The solution obtained in step (4) is subjected to photopolymerization under ultraviolet light to prepare a polymerizable deep eutectic gel.
[0056] Example 4
[0057] This embodiment provides a method for preparing a polymerizable deep eutectic gel, which comprises the following steps:
[0058] (1) 25 g of choline chloride and 25.7 g of acrylic acid solution were mixed, heated and stirred at 90° C. for 3 h until the solution became transparent, to obtain a polymerizable deep eutectic solvent;
[0059] (2) adding 2 g of rice husk into 40 ml of a polymerizable deep eutectic solvent and heating and stirring at 100 °C for 90 min to extract lignin from the rice husk;
[0060] (3) centrifuging the solution obtained in step (2) and extracting the supernatant;
[0061] (4) adding photoinitiator 2959 to the supernatant obtained in step (3), wherein the mass volume ratio of photoinitiator 2959 to supernatant is 4:12675, and stirring for 5 minutes in a dark environment;
[0062] (5) The solution obtained in step (4) is subjected to photopolymerization under ultraviolet light to prepare a polymerizable deep eutectic gel.
[0063] Example 5
[0064] This embodiment provides a method for preparing a polymerizable deep eutectic gel, which comprises the following steps:
[0065] (1) 25 g of choline chloride and 25.7 g of acrylic acid solution were mixed, heated and stirred at 90° C. for 3 h until the solution became transparent, to obtain a polymerizable deep eutectic solvent;
[0066] (2) adding 2 g of rice husk into 40 ml of a polymerizable deep eutectic solvent and heating and stirring at 100 °C for 120 min to extract lignin from the rice husk;
[0067] (3) centrifuging the solution obtained in step (2) and extracting the supernatant;
[0068] (4) adding photoinitiator 2959 to the supernatant obtained in step (3), wherein the mass volume ratio of photoinitiator 2959 to supernatant is 4:12675, and stirring for 5 minutes in a dark environment;
[0069] (5) The solution obtained in step (4) is subjected to photopolymerization under ultraviolet light to prepare a polymerizable deep eutectic gel.
[0070] Comparative Example 1
[0071] This comparative example provides a method for preparing a polymerizable deep eutectic gel, which comprises the following steps:
[0072] (1) 25 g of choline chloride and 25.7 g of acrylic acid solution were mixed, heated and stirred at 90° C. for 3 h until the solution became transparent, to obtain a polymerizable deep eutectic solvent;
[0073] (2) adding a photoinitiator to the polymerizable deep eutectic solvent obtained in step (1), wherein the mass volume ratio of the photoinitiator 2959 to the polymerizable deep eutectic solvent is 4:12675, and stirring for 5 minutes in a light-proof condition;
[0074] (3) The solution obtained in step (2) is subjected to photopolymerization under ultraviolet light to prepare a gel material.
[0075] Comparative Example 2
[0076] This comparative example provides a method for preparing a polymerizable deep eutectic gel, which comprises the following steps:
[0077] (1) 25 g of choline chloride and 25.7 g of acrylic acid solution were mixed, heated and stirred at 90° C. for 3 h until the solution became transparent, to obtain a polymerizable deep eutectic solvent;
[0078] (2) adding 2 g of rice husk into 40 ml of a polymerizable deep eutectic solvent and heating and stirring at 100 °C for 60 min to extract lignin from the rice husk;
[0079] (3) centrifuging the solution obtained in step (2) and extracting the supernatant;
[0080] (4) The solution obtained in step (3) is subjected to photopolymerization under ultraviolet light to prepare a gel material.
[0081] The sensing performance of the polymerizable deep eutectic gel prepared in Example 3 was tested. Figure 2 It can be seen that it can detect the relative current changes when the finger is bent at different angles; according to the attached Figure 3 It can be seen that it can detect the relative current changes when the wrist is bent at the same angle; Figure 4 As shown, it can detect the relative current changes when the knees are bent at the same angle. Therefore, the polymerizable deep eutectic gel provided by the present invention is applied to flexible sensors and can show excellent sensitivity. It can not only detect small changes in human limbs, such as bending fingers at different angles, but also detect limb movements with larger amplitudes, such as bending wrists and knees.
[0082] The mechanical properties, conductivity and adhesion of the gel materials prepared in Examples 1-5 and Comparative Example 1 were tested. The gel in Comparative Example 2 lacked a photoinitiator, which resulted in the inability to form the material, so its specific properties could not be tested. Among them, the mechanical strength was tested using a universal mechanical testing machine, the conductivity was measured using an electrochemical workstation, and the adhesion strength on the metal plate was detected using the overlap shear method. As shown in Table 1, the tensile strength and elongation at break of the gels of Examples 1-5 are significantly better than those of Comparative Example 1, especially the gel material of Example 3, which has the most excellent mechanical properties, with a tensile strength of up to 1210.9 KPa and an elongation at break of up to 1445.8%. In addition, as shown in Table 2, the conductivity and adhesion strength of the gels of Examples 1-5 are also significantly higher than those of Comparative Example 1, especially the gel material of Example 3, with a conductivity of up to 43.0×10 -3 S / m, and the adhesion strength is as high as 61.5 KPa. Therefore, the polymerizable deep eutectic gel prepared by the method provided by the present invention has excellent mechanical strength, adhesion, and conductivity, and can be recycled.
[0083] Table 1 Mechanical strength test results
[0084]
[0085] Table 2 Conductivity and adhesion strength test results
[0086] Serial number Conductivity (S / m, 25℃) Adhesion strength / KPa Comparative Example 1 <![CDATA[19.3×10 -3 ]]> 28.2 Example 1 <![CDATA[28.4×10 -3 ]]> 31.4 Example 2 <![CDATA[33.0×10 -3 ]]> 34.5 Example 3 <![CDATA[43.0×10 -3 ]]> 61.5 Example 4 <![CDATA[40.0×10 -3 ]]> 57.0 Example 5 <![CDATA[36.4×10 -3 ]]> 28.7
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a polymerizable deep eutectic gel, characterized in that: The rice husk is added into a polymerizable deep eutectic solvent, and the lignin in the rice husk is extracted by heating and stirring; the supernatant is then extracted by centrifugation, a photoinitiator is added into the supernatant, and photopolymerization is performed under ultraviolet light to obtain a polymerizable deep eutectic gel; The mass volume ratio of rice husk to polymerizable deep eutectic solvent is 1 g:20 ml; After adding rice husk into the polymerizable deep eutectic solvent, the heating and stirring time is 30-90 minutes at a temperature of 90-100°C; The choline chloride and acrylic acid solution are mixed, heated and stirred until the solution becomes transparent, thereby obtaining a polymerizable deep eutectic solvent; The molar ratio of choline chloride to acrylic acid solution is 1:2; The concentration of the acrylic acid solution is 98%.
2. The method for preparing a polymerizable deep eutectic gel according to claim 1, characterized in that: After the choline chloride and acrylic acid solution are mixed, the heating and stirring time is 3-4 hours at a temperature of 90-95°C.
3. The method for preparing a polymerizable deep eutectic gel according to claim 1, characterized in that: The mass volume ratio of the photoinitiator to the supernatant is 4g:12675ml.
4. The method for preparing a polymerizable deep eutectic gel according to claim 1, characterized in that: After adding the photoinitiator to the supernatant, stir for 5-10 minutes in a dark environment and then perform photopolymerization.
5. The polymerizable deep eutectic gel obtained by the method for preparing the polymerizable deep eutectic gel according to any one of claims 1 to 4.
6. Use of the polymerizable deep eutectic gel according to claim 5 in flexible sensors.