Separation and adsorption material for enriching sedimentary clay lithium ore and extracting lithium and preparation method of separation and adsorption material
By mixing the polyamic acid solution with HTO to make a spinning liquid and imidizing it, HTO/polyimide nanofibers are formed, which solves the problem of poor circulation and adsorption performance of lithium ion sieve and achieves high efficiency Lithium ion extraction and recycling.
Patent Information
- Application Number
- CN202411121874.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The existing lithium ion sieve has poor circulation and adsorption performance, and the dissolution loss of lithium manganese oxides during the acid leach recovery process is high, and the circulation stability performance is poor, making it difficult to achieve efficient lithium ion extraction.
The spinning liquid is made by mixing polyamic acid solution with HTO and HTO. The HTO/polyimide nanofiber is formed through imidation treatment. The complex polymer network forms a separation adsorbent material with good mechanical properties, which improves the separation adsorbent material. corrosion resistance and cycle performance.
The cyclic performance and corrosion resistance of extracted lithium-separated adsorbent materials are improved, the stability of the HTO ion sieve structure is maintained, the adsorption and desorption capacity of lithium ions is enhanced, and the corrosion loss during the pickling and desorption process is reduced.
Smart Images

Figure CN119016033A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ore extraction, and specifically refers to an adsorption material and a preparation method for enriching sedimentary clay lithium ore and extracting lithium. Background Art
[0002] Lithium metal has high electrochemical activity and is the lightest alkali metal. It also has physical and chemical properties such as high reduction and oxidation potential and high specific heat capacity. With the development of emerging industries, lithium metal has been widely used in technical fields such as batteries, electronic information equipment, ceramics, and aerospace. The extraction of lithium elements mainly includes the following methods: solvent extraction, precipitation crystallization, adsorption, and membrane separation. Among them, precipitation crystallization is widely used in the field of lithium extraction technology and the technology is relatively mature. Due to the poor selectivity of this method, it is only applicable to systems with low magnesium-to-lithium ratios and fewer impurities. Solvent extraction has high selectivity for lithium elements and is widely used in salt lake systems, but solvent extraction is prone to produce three-phase waste, and the use of organic solvents is prone to corrode industrial equipment. Membrane separation methods mainly include selective electrodialysis, nanofiltration membranes, ion imprinting membranes, and membrane capacitor deionization, which have the advantages of high efficiency and environmental protection, but are difficult to promote due to defects such as high energy consumption and high cost. Adsorption is to select or design and synthesize adsorption materials that have the ability to recognize lithium ions, and use specific physical and chemical effects to achieve selective separation and recovery of lithium ions. Adsorption materials are the core of adsorption lithium extraction; ideal adsorption materials should have high selectivity , high stability and high adsorption capacity. According to the properties of the adsorbent, it can be roughly divided into organic adsorption materials, inorganic adsorption materials and composite adsorption materials. Among them, organic adsorption materials include crown ethers, calixarene, etc., and the suspension adsorption of lithium ions is achieved by regulating the crown ether hole size and the coordination with lithium ions; the process of extracting lithium from inorganic materials is mainly to saturate the lithium ions with adsorption, and then separate the lithium ions and the adsorption material by immersing the adsorbent in water, and use a precipitant to remove calcium, magnesium and other ions in the lithium-containing solution. After concentration, sodium carbonate is added to precipitate lithium to achieve lithium carbonate. In the production of products, inorganic adsorbents mainly include aluminum-based adsorbents, lithium ion sieves, natural minerals and carbon materials, among which natural minerals and carbon materials can combine with active metal ions through the active sites on the surface of the materials, which leads to poor selective adsorption of lithium ions. Lithium ion sieve adsorbents mainly include lithium manganese oxide and lithium titanium oxide. Lithium manganese oxide has a high dissolution loss during acid leaching to recover lithium, poor cyclic stability, and low reusability. Lithium titanium oxide and aluminum-based adsorbents have good stability, but they also have problems such as difficult desorption and slow solid-phase mass transfer. Summary of the invention
[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a separation adsorption material and a preparation method for enriching and extracting lithium from sedimentary clay lithium ore. In order to solve the problem of poor cycle performance and adsorption performance of lithium ion sieve, the present invention mixes a polyamic acid solution with HTO to form a spinning solution, and after the fiber is made, it is subjected to imidization treatment to form HTO / polyimide nanofibers. A separation adsorption material with good mechanical properties is formed through a complex polymer network, the corrosion resistance of the separation adsorption material is improved, the structural decomposition of the HTO ion sieve structure can be maintained during the cyclic use, and the cycle performance of the lithium extraction separation adsorption material is improved.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0005] The present invention also provides a method for preparing a separation adsorption material for enriching and extracting lithium from sedimentary clay lithium ore, which specifically comprises the following steps:
[0006] S1. Disperse diaminodiphenyl ether in NMP solvent, mix well, place in ice water bath, add 3,5-diaminobenzoic acid, add 4,4'-biphenyl ether dianhydride, stir at 300 rpm, continue stirring for 8-12 hours, add triethylamine, continue mixing for 3-5 hours, and obtain a polyamic acid solution with a solid content of 10%-15%;
[0007] Preferably, in step S1, the raw materials for preparing the polyamic acid solution are composed of the following parts by weight: 0.45-0.6 parts of diaminodiphenyl ether, 0.05-0.15 parts of 3,5-diaminobenzoic acid, and 1 part of 4,4-biphenyl ether dianhydride;
[0008] Preferably, in step S1, the mass concentration of the diaminodiphenyl ether in the NMP solvent is 25-60 g / L;
[0009] S2, dissolving lithium acetate in deionized water, adding CTAB and mixing evenly, dissolving tetrabutyl titanate in anhydrous ethanol, adding glacial acetic acid, placing on a magnetic stirrer and mixing evenly at a speed of 180-220 rpm, adding dropwise to the lithium acetate solution, stirring for 15-20 min at room temperature, raising the temperature to 60-70° C. and stirring until a milky white sol is generated, standing at room temperature for 24 h for aging treatment, drying at 80-100° C., and grinding to obtain an LTO precursor;
[0010] Preferably, in step S2, the mass ratio between tetrabutyl titanate and lithium acetate is 4:1-1.2;
[0011] Preferably, in step S2, the mass concentration of lithium acetate in deionized water is 0.08-0.1 g / mL, and the added mass of CTAB is 4%-6% of the mass of lithium acetate;
[0012] Preferably, in step S2, the mass concentration of tetrabutyl titanate in anhydrous ethanol is 0.2-0.4 g / mL, and the volume ratio between glacial acetic acid and anhydrous ethanol is 2:1-1.2;
[0013] S3, placing the LTO precursor prepared in step S2 in a high-temperature tube furnace, and calcining it at 700-900° C. for 3-5 hours, and obtaining LTO powder after calcination;
[0014] S4, dispersing the LTO powder prepared in step S3 in a hydrochloric acid solution, raising the reaction temperature to 60-70°C, stirring the reaction at 150 rpm for 20-30 hours, filtering, washing with deionized water, and drying and grinding the HTO powder;
[0015] Preferably, in step S4, the mass concentration of the LTO powder in the hydrochloric acid solution is 2.5-5 g / L, and the molar concentration of hydrochloric acid in the hydrochloric acid solution is 0.1-0.2 mol / L;
[0016] S5, adding the HTO powder prepared in step S4 to NMP solvent, stirring and dispersing at 200-250 rpm and 25° C. for 3-5 hours, adding the polyamic acid solution prepared in step S1 after uniform dispersion, raising the temperature to 50-60° C., continuing to stir and mix for 8-10 hours, and vacuum degassing to obtain HTO / polyamic acid spinning solution;
[0017] Preferably, in step S5, the mass concentration of the HTO powder in the DMA solvent is 20-40 g / L;
[0018] Preferably, in step S5, the volume ratio between the HTO dispersion and the polyamic acid solution is 1:1;
[0019] S6, transferring the HTO / polyamic acid spinning solution prepared in step S5 into a syringe, and delivering it to an electrospinning machine through a needle with an inner diameter of 0.51 mm at a fixed flow rate of 2 mL / h, the voltage between the needle and the collector is controlled at 22-25 kV, and the distance between the needle and the collector is 150 mm, placing the spun fiber in a coagulation bath solution, immersing it in the coagulation bath solution for chemical imidization treatment for 12-18 hours, and then drying it through supercritical CO2 to obtain a lithium extraction separation adsorption material;
[0020] Preferably, in step S6, the coagulation bath solution comprises the following components in volume ratio: 2 parts of acetone, 0.1-0.2 parts of acetic anhydride, and 0.1-0.2 parts of triethylamine.
[0021] The present invention also provides a separation adsorption material for enriching sedimentary clay lithium ore and extracting lithium prepared according to the above method;
[0022] Preferably, the method for extracting lithium from the lithium separation adsorption material comprises the following steps:
[0023] ① Crushing sedimentary clay samples, screening and grading, and then crushing the particles of +3mm to obtain lithium ore particles with a particle size of less than 3mm;
[0024] ② The lithium ore particles prepared in step ① are scrubbed so that the proportion of fine ore particles with a particle size of -0.075 mm exceeds 66.33%, and then classified to obtain classified concentrate 1 and tailings 1;
[0025] ③ The classified concentrate 1 obtained in step ② is subjected to cyclone classification to obtain a classified concentrate 2 and tailings 2;
[0026] ④ Sample 10 g of the graded concentrate 2 obtained in step ③ and place it in a beaker, prepare a hydrochloric acid solution with a mass concentration of 30%, add it to the graded concentrate 2, and place it on a magnetic stirrer and stir it at a speed of 200-250 rpm for 90-120 min, filter it, separate the filtrate and the precipitate, the filtrate is a lithium-containing leaching solution, wash the precipitate with deionized water until it is neutral, and dry it to obtain a lithium-rich mineral;
[0027] ⑤ The lithium-containing leaching solution separated in step ④ is adjusted to pH 10-12, and the lithium extraction separation adsorption material is added and mixed, and stirred at a speed of 150 rpm in a constant temperature water bath at 25° C., and after stirring and reacting for 24 hours, filtered, and the precipitate is collected as a lithium-rich material.
[0028] The beneficial effects achieved by the present invention are as follows:
[0029] The present invention provides a separation adsorption material for enriching and extracting lithium from sedimentary clay lithium ore and a preparation method thereof. In the present invention, a polyamic acid solution is mixed with HTO to form a spinning solution, and after being made into fibers, an imidization treatment is performed to form HTO / polyimide nanofibers. A separation adsorption material with good mechanical properties is formed through a complex polymer network, the corrosion resistance of the separation adsorption material is improved, the structural decomposition of the HTO ion sieve structure can be maintained during the cyclic use process, and the cyclic performance of the lithium extraction separation adsorption material is improved; the present invention adopts diaminodiphenyl ether and 4,4-biphenyl ether dianhydride as reaction monomers of polyimide, replaces part of the diamine monomers with 3,5-diaminobenzoic acid, and introduces The carboxyl group can be well combined with the HTO ion sieve through intermolecular forces, so that the HTO powder can be evenly distributed in the polyamic acid solution. After the spinning process, the formed fiber is chemically imidized, and the HTO is evenly distributed on the surface of the polyimide fiber, providing support for the HTO ion sieve structure. During the adsorption / desorption process, the content of the Ti element is maintained, and the corrosion of the HTO ion sieve structure during the acid washing and desorption process is increased, thereby improving the recycling performance of the HTO ion sieve. Since the lithium ore is fine in particle size and is very easy to be muddy, the scrubbing process used in the present invention can effectively prevent mud from being caused by over-grinding, and also create good particle size conditions for the subsequent classification process to treat gangue minerals such as quartz, calcium salts and pyrite. The cyclone classification process can efficiently eject a portion of the gangue minerals, reduce the feed amount of the subsequent acid leaching process, and reduce the amount of hydrochloric acid used. In the hydrochloric acid separation process, chloride ions (Cl-) act as a catalyst. Chloride ions react with hydrogen ions (H + ) react to generate chloride ion free radicals (Cl·), which are highly active oxidants, making the reaction between gangue minerals and hydrochloric acid solution more rapid and thorough, accelerating the dissolution rate of gangue minerals; and promoting the metal ions (Me 2+ ) leaves the solid phase, further reducing the interference of gangue minerals in the lithium enrichment process, while it itself does not change or consume, so it can be recycled and reused. Through classification and chemical separation processes, gangue minerals in lithium ore can be effectively removed and the concentrate grade can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is an infrared spectrum image of the lithium extraction and separation adsorption material prepared in Example 1 of the present invention;
[0031] Figure 2 This is a SEM image of the lithium extraction and separation adsorption material prepared in Example 1 of the present invention;
[0032] Figure 3 The equilibrium adsorption capacity result diagram of the separation adsorption materials prepared in Examples 1-3 and Comparative Examples 1-3;
[0033] Figure 4 The cycle performance results of the lithium extraction and separation adsorption materials prepared in Examples 1-3 and Comparative Examples 1-3 are shown;
[0034] Figure 5 This is a process flow chart for lithium ore enrichment and lithium extraction described in Example 1 of the present invention.
[0035] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0037] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0038] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials and test strains used in the following examples are purchased from commercial channels unless otherwise specified.
[0039] Example 1
[0040] This embodiment provides a method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material, which specifically includes the following steps:
[0041] S1. Accurately weigh 1.35 g of diaminodiphenyl ether and place it in a flask, add 50 mL of NMP solvent and mix until the solution is completely dissolved, transfer to an ice water bath environment for stirring, accurately weigh 3.0 g of 4,4'-biphenyl ether dianhydride and 0.45 g of 3,5-diaminobenzoic acid and add them to the reaction system, stir and react at 300 rpm for 10 hours, add 3 mL of triethylamine, continue stirring for 4 hours, and obtain a polyamic acid solution, and measure its solid content to be 10.5%;
[0042] S2. Accurately weigh 2g of lithium acetate and place it in 20mL of deionized water, add 0.1g of CTAB and mix evenly to form a uniform solution; accurately weigh 8g of tetrabutyl titanate and place it in 20mL of anhydrous ethanol, add 10mL of glacial acetic acid and mix evenly, then mix at 25°C and 200rpm, add lithium acetate solution dropwise, continue mixing for 20min, increase the temperature to 65°C and mix until the reaction system becomes a milky white uniform sol, after the reaction temperature is cooled to room temperature, place the solvent at room temperature for 24h, place it in a 100°C oven for drying, and grind it evenly to obtain an LTO precursor;
[0043] S3, placing the LTO precursor prepared in step S2 in a high-temperature tube furnace, calcining it at 800° C. for 4 hours, and then cooling it to room temperature to obtain LTO powder;
[0044] S4, accurately weighing 5 g of the LTO powder prepared in step S3 and placing it in a container, adding 1 L of 0.1 mol / L HCl solution, fully dispersing the LTO powder in the HCl solution at a speed of 150 rpm, raising the reaction temperature to 65° C., acid-washing the LTO powder, reacting for 24 hours, filtering, washing the precipitate with deionized water until the washing solution is neutral, drying, and grinding evenly to obtain HTO powder;
[0045] S5. Accurately weigh 1 g of the HTO powder prepared in step S4 and place it in 50 mL of NMP solvent. Stir at 200 rpm and 25° C. for 3 h to fully disperse the HTO powder in the NMP solvent. Add the polyamic acid solution prepared in step S1 to the HTO / NMP dispersion, stir and mix, raise the reaction temperature to 50° C., continue stirring and reacting for 10 h, wait for the reaction system to cool to room temperature, and perform vacuum degassing to obtain an HTO / polyamic acid spinning solution.
[0046] S6. The HTO / polyamic acid spinning solution prepared in step S5 is transferred to a syringe, and sent to an electrospinning machine through a needle with an inner diameter of 0.51 mm at a fixed flow rate of 2 mL / h, the voltage between the needle and the collector is controlled at 22-25 kV, and the distance between the needle and the collector is 150 mm. 1 L of acetone, 50 mL of acetic anhydride and 50 mL of triethylamine are mixed to prepare a coagulation bath solution, the spun fiber is placed in the coagulation bath solution, soaked for 18 h, filtered, washed with deionized water and anhydrous ethanol, dried with supercritical CO2, and the coagulation bath solution and washing liquid are removed to obtain a lithium extraction separation adsorption material.
[0047] This embodiment also provides a separation adsorption material for extracting lithium from sedimentary clay lithium ore prepared according to the above method;
[0048] The method for extracting lithium separation adsorption material for lithium extraction specifically comprises the following steps:
[0049] ① Crushing sedimentary clay samples, screening and grading, and then crushing the particles of +3mm to obtain lithium ore particles with a particle size of less than 3mm;
[0050] ② The lithium ore particles prepared in step ① are scrubbed so that the proportion of fine ore particles with a particle size of -0.075 mm exceeds 66.33%, and then classified to obtain classified concentrate 1 and tailings 1;
[0051] ③ The classified concentrate 1 obtained in step ② is subjected to cyclone classification to obtain a classified concentrate 2 and tailings 2;
[0052] ④ Sample 10 g of the graded concentrate 2 obtained in step ③ and place it in a beaker, prepare a hydrochloric acid solution with a mass concentration of 30%, add it to the graded concentrate 2 according to a solid-liquid ratio of 1:4, and place it on a magnetic stirrer and stir it at 250 rpm for 120 minutes, filter, separate the filtrate and the precipitate, the filtrate is a lithium-containing leaching solution, wash the precipitate with deionized water until neutral, and dry it to obtain a lithium-rich mineral;
[0053] ⑤ Adjust the pH of the lithium-containing leaching solution separated in step ④ to 12, add 0.4 g / L of lithium extraction separation adsorption material to mix, stir at 150 rpm under a constant temperature water bath at 25° C., stir the reaction for 24 hours, filter, and collect the precipitate as a lithium-rich material.
[0054] Example 2
[0055] This embodiment provides a method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material, which specifically includes the following steps:
[0056] S1. Accurately weigh 1.5 g of diaminodiphenyl ether and place it in a flask, add 30 mL of NMP solvent and mix until the solution is completely dissolved, transfer to an ice water bath environment for stirring, accurately weigh 3.0 g of 4,4'-biphenyl ether dianhydride and 0.3 g of 3,5-diaminobenzoic acid and add them to the reaction system, stir and react at 300 rpm for 12 hours, add 3 mL of triethylamine, continue stirring for 5 hours, and obtain a polyamic acid solution, and measure its solid content to be 12.2%;
[0057] S2. Accurately weigh 1.2g of lithium acetate and place it in 15mL of deionized water, add 0.5g of CTAB and mix evenly to form a uniform solution, accurately weigh 4g of tetrabutyl titanate and place it in 20mL of anhydrous ethanol, add 12mL of glacial acetic acid and mix evenly, then mix at 25°C and 180rpm, add lithium acetate solution dropwise, continue mixing for 15min, raise the temperature to 70°C and mix until the reaction system becomes a milky white uniform sol, after the reaction temperature is cooled to room temperature, place the solvent at room temperature for 24h, place it in a 100°C oven for drying, and grind it evenly to obtain an LTO precursor;
[0058] S3, placing the LTO precursor prepared in step S2 in a high-temperature tube furnace, calcining it at 900° C. for 3 h, and then cooling it to room temperature to obtain LTO powder;
[0059] S4, accurately weighing 2.5 g of the LTO powder prepared in step S3 and placing it in a container, adding 1 L of 0.2 mol / L HCl solution, fully dispersing the LTO powder in the HCl solution at a speed of 150 rpm, raising the reaction temperature to 60° C., acid-washing the LTO powder, reacting for 20 hours, filtering, washing the precipitate with deionized water until the washing solution is neutral, drying, and grinding evenly to obtain HTO powder;
[0060] S5. Accurately weigh 1.2 g of the HTO powder prepared in step S4 and place it in 30 mL of NMP solvent. Stir at 250 rpm and 25° C. for 4 h to fully disperse the HTO powder in the NMP solvent. Add the polyamic acid solution prepared in step S1 to the HTO / NMP dispersion, stir and mix, raise the reaction temperature to 55° C., continue stirring and reacting for 9 h, wait for the reaction system to cool to room temperature, and perform vacuum degassing to obtain an HTO / polyamic acid spinning solution.
[0061] S6. The HTO / polyamic acid spinning solution prepared in step S5 is transferred to a syringe and sent to an electrospinning machine through a needle with an inner diameter of 0.51 mm at a fixed flow rate of 2 mL / h. The voltage between the needle and the collector is controlled at 22-25 kV, and the distance between the needle and the collector is 150 mm. 1 L of acetone, 50 mL of acetic anhydride and 50 mL of triethylamine are mixed to prepare a coagulation bath solution. The spun fiber is placed in the coagulation bath solution, soaked for 12 h, filtered, washed with deionized water and anhydrous ethanol, dried with supercritical CO2, and the coagulation bath solution and washing liquid are removed to obtain a lithium extraction separation adsorption material.
[0062] This embodiment also provides a separation adsorption material for extracting lithium from sedimentary clay lithium ore prepared according to the above method;
[0063] The method for extracting lithium separation adsorption material for lithium extraction specifically comprises the following steps:
[0064] ① Crushing sedimentary clay samples, screening and grading, and then crushing the particles of +3mm to obtain lithium ore particles with a particle size of less than 3mm;
[0065] ② The lithium ore particles prepared in step ① are scrubbed so that the proportion of fine ore particles with a particle size of -0.075 mm exceeds 66.33%, and then classified to obtain classified concentrate 1 and tailings 1;
[0066] ③ The classified concentrate 1 obtained in step ② is subjected to cyclone classification to obtain a classified concentrate 2 and tailings 2;
[0067] ④ Sample 10 g of the graded concentrate 2 obtained in step ③ and place it in a beaker, prepare a hydrochloric acid solution with a mass concentration of 30%, add it to the graded concentrate 2 according to a solid-liquid ratio of 1:4, and place it on a magnetic stirrer and stir it at 220 rpm for 90 minutes, filter it, separate the filtrate and the precipitate, the filtrate is a lithium-containing leaching solution, wash the precipitate with deionized water until neutral, and dry it to obtain a lithium-rich mineral;
[0068] ⑤ Adjust the pH of the lithium-containing leaching solution separated in step ④ to 11, add 0.4 g / L of lithium extraction separation adsorption material to mix, stir at 150 rpm under a constant temperature water bath at 25° C., stir the reaction for 24 hours, filter, and collect the precipitate as a lithium-rich material.
[0069] Example 3
[0070] This embodiment provides a method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material, which specifically includes the following steps:
[0071] S1. Accurately weigh 1.8 g of diaminodiphenyl ether and place it in a flask, add 30 mL of NMP solvent and mix until the solution is completely dissolved, transfer to an ice water bath environment for stirring, accurately weigh 3.0 g of 4,4'-biphenyl ether dianhydride and 0.15 g of 3,5-diaminobenzoic acid and add them to the reaction system, stir and react at 300 rpm for 8 hours, add 3 mL of triethylamine, continue stirring for 3 hours, and obtain a polyamic acid solution, and measure its solid content to be 14.6%;
[0072] S2. Accurately weigh 2g of lithium acetate and place it in 20mL of deionized water, add 0.3g of CTAB and mix evenly to form a uniform solution, accurately weigh 8g of tetrabutyl titanate and place it in 20mL of anhydrous ethanol, add 10mL of glacial acetic acid and mix evenly, then mix at 25°C and 220rpm, add lithium acetate solution dropwise, continue mixing for 15min, raise the temperature to 60°C and mix until the reaction system becomes a milky white uniform sol, after the reaction temperature is cooled to room temperature, place the solvent at room temperature for 24h, place it in a 100°C oven for drying, and grind it evenly to obtain an LTO precursor;
[0073] S3, placing the LTO precursor prepared in step S2 in a high-temperature tube furnace, calcining it at 700° C. for 5 h, and then cooling it to room temperature to obtain LTO powder;
[0074] S4, accurately weighing 4 g of the LTO powder prepared in step S3 and placing it in a container, adding 1 L of 0.15 mol / L HCl solution, fully dispersing the LTO powder in the HCl solution at a speed of 150 rpm, raising the reaction temperature to 65° C., acid-washing the LTO powder, reacting for 24 hours, filtering, washing the precipitate with deionized water until the washing solution is neutral, drying, and grinding evenly to obtain HTO powder;
[0075] S5. Accurately weigh 1.5 g of the HTO powder prepared in step S4 and place it in 45 mL of NMP solvent. Stir at 230 rpm and 25 ° C for 5 h to fully disperse the HTO powder in the NMP solvent. Add the polyamic acid solution prepared in step S1 to the HTO / NMP dispersion, stir and mix, increase the reaction temperature to 60 ° C, continue stirring and reacting for 8 h, wait for the reaction system to cool to room temperature, and perform vacuum degassing to obtain HTO / polyamic acid spinning solution.
[0076] S6. The HTO / polyamic acid spinning solution prepared in step S5 is transferred to a syringe, and sent to an electrospinning machine through a needle with an inner diameter of 0.51 mm at a fixed flow rate of 2 mL / h, the voltage between the needle and the collector is controlled at 22-25 kV, and the distance between the needle and the collector is 150 mm. 1 L of acetone, 50 mL of acetic anhydride and 50 mL of triethylamine are mixed to prepare a coagulation bath solution, the spun fiber is placed in the coagulation bath solution, soaked for 15 h, filtered, washed with deionized water and anhydrous ethanol, dried with supercritical CO2, and the coagulation bath solution and washing liquid are removed to obtain a lithium extraction separation adsorption material.
[0077] This embodiment also provides a separation adsorption material for extracting lithium from sedimentary clay lithium ore prepared according to the above method;
[0078] The method for extracting lithium separation adsorption material for lithium extraction specifically comprises the following steps:
[0079] ① Crushing sedimentary clay samples, screening and grading, and then crushing the particles of +3mm to obtain lithium ore particles with a particle size of less than 3mm;
[0080] ② The lithium ore particles prepared in step ① are scrubbed so that the proportion of fine ore particles with a particle size of -0.075 mm exceeds 66.33%, and then classified to obtain classified concentrate 1 and tailings 1;
[0081] ③ The classified concentrate 1 obtained in step ② is subjected to cyclone classification to obtain a classified concentrate 2 and tailings 2;
[0082] ④ Sample 10 g of the graded concentrate 2 obtained in step ③ and place it in a beaker, prepare a hydrochloric acid solution with a mass concentration of 30%, add it to the graded concentrate 2 according to a solid-liquid ratio of 1:4, and place it on a magnetic stirrer and stir it at 200 rpm for 120 minutes, filter it, separate the filtrate and the precipitate, the filtrate is a lithium-containing leaching solution, wash the precipitate with deionized water until it is neutral, and dry it to obtain a lithium-rich mineral;
[0083] ⑤ Adjust the pH of the lithium-containing leaching solution separated in step ④ to 10, add 0.4 g / L of lithium extraction separation adsorption material to mix, stir at 150 rpm under a constant temperature water bath at 25° C., stir the reaction for 24 hours, filter, and collect the precipitate as a lithium-rich material.
[0084] Comparative Example 1
[0085] This comparative example provides a lithium extraction separation adsorption material and a preparation method thereof, which differs from Example 1 only in that, in step S1, the raw materials for preparing the polyamic acid solution do not include 3,5-diaminobenzoic acid, and are replaced by two parts of diaminodiphenyl ether, and the remaining components, component contents, and preparation methods are the same as those in Example 1.
[0086] Comparative Example 2
[0087] This comparative example provides a lithium extraction separation adsorption material and a preparation method thereof, which is different from Example 1 only in that the preparation method does not include steps S1, S5, and S6, that is, the lithium extraction separation adsorption material is HTO powder, and the remaining components, component contents, and preparation methods are the same as those in Example 1.
[0088] Comparative Example 3
[0089] This comparative example provides a lithium extraction separation material and a preparation method thereof, which differs from Example 1 only in that the preparation method does not include step S1, and in step S5, the polyamic acid solution is replaced with a polyimide / NMP solution with the same solid content, and the remaining components, component contents, and preparation method are the same as those in Example 1.
[0090] Experimental Example 1
[0091] In this experimental example, the lithium extraction and separation adsorption material prepared in Example 1 was subjected to infrared spectroscopy analysis using an IRTracer-100 Fourier transform infrared spectrometer and a potassium bromide tablet method. The scanning beam range was 4000-500 cm -1 .
[0092] Figure 1 This is the infrared spectrum image of the lithium extraction and separation adsorption material prepared in Example 1 of the present invention. As shown in the figure, at 1790-1770cm -1 and 1740-1710cm -1 The characteristic peak of -C=O appears at 1620-1600cm, indicating that the material contains a typical imine group, while the characteristic peak of the amide group does not appear, indicating that the material has completed imidization. -1 The characteristic peak of carbonyl hydrogen appears at 680-650cm -1 The appearance of the characteristic peak of Ti-O indicates that HTO-doped polyimide fiber material is formed after HTO and polyamic acid solution are spun and chemically imidized.
[0093] Experimental Example 2
[0094] In this experimental example, the microscopic morphology of the lithium extraction and separation adsorption material prepared in Example 1 was observed. The morphology of the lithium extraction and separation adsorption material prepared in Example 1 was observed using a SU8010 field emission electron scanning microscope. The sample material was placed in liquid nitrogen for brittle fracture and then attached to a sample table for gold spraying.
[0095] Figure 2 This is a SEM image of the lithium extraction and separation adsorption material prepared in Example 1 of the present invention. As shown in the figure, the HTO powder material is evenly dispersed on the polyimide fiber, and there are wide gaps between the fibers and they are intertwined to form a network structure, which can provide conditions for sufficient contact between lithium ions and HTO, thereby improving the material's adsorption performance for lithium ions.
[0096] Experimental Example 3
[0097] In this experimental example, the adsorption performance of the lithium extraction and separation adsorption materials prepared in Examples 1-3 and Comparative Examples 1-3 was measured, and a LiCl solution was prepared, wherein the Li+ concentration was 100 mg / L and the pH was 6.5. 0.1 g of the extraction and separation adsorption materials prepared in Examples 1-3 and Comparative Examples 1-3 was dispersed in 100 mL of the LiCl solution, and stirred at a speed of 150 rpm at room temperature. After adsorption for 24 hours, the equilibrium adsorption capacity of the lithium extraction and separation material was measured;
[0098] Figure 3The equilibrium adsorption capacity result diagram of the separation adsorption materials prepared in Examples 1-3 and Comparative Examples 1-3 is shown in the figure. As shown in the figure, Comparative Example 2 is the adsorption capacity of HTO powder for lithium ions, and the adsorption equilibrium capacity is 28.6 mg / g. The adsorption equilibrium capacity of the lithium extraction separation adsorption materials prepared in Examples 1-3 is 25.6 mg / g, 23.8 mg / g, and 24.3 mg / g, indicating that the adsorption capacity of the lithium extraction separation adsorption material prepared by the present invention for lithium ions is equivalent to the adsorption capacity of the simple HTO lithium ion sieve. In the separation adsorption material described in Comparative Example 1, no polymer monomer having a carboxyl group is introduced into the polymer, which reduces the hydrophilicity of the separation adsorption material, resulting in the obstruction of the circulation of the lithium ion solution in the polyimide fiber, resulting in a reduction in the contact area between HTO and lithium ions, and reducing the adsorption capacity for lithium ions; in Comparative Example 3, polyimide is directly mixed with HTO and then spun, and the polyimide fiber has a poor affinity for HTO, resulting in the agglomeration of HTO, thereby weakening the lithium ion adsorption performance of the material.
[0099] Figure 4 The cycle performance results of the lithium extraction and separation adsorption materials prepared in Examples 1-3 and Comparative Examples 1-3 are shown in the figure. As shown in the figure, the cycle performance of the lithium extraction and separation adsorption materials prepared in Examples 1-3 is relatively high. After 8 cycles, the adsorption capacity for lithium ions can still reach 20-22 mg / g. Although the initial adsorption performance of Comparative Example 2 is relatively high, the structure of HTO changes during repeated adsorption and elution cycles, resulting in a decrease in the adsorption capacity for lithium ions. The adsorption capacity for lithium ions in Comparative Example 1 drops to 11.2 mg / g after 8 cycles. After 6 cycles, the material in Comparative Example 3 is completely passivated and has almost no adsorption performance for lithium ions. This shows that the lithium extraction and separation adsorption material prepared by the present invention can provide efficient combination of HTO and polyimide fibers to form a fiber material with uniform HTO distribution, provide support for HTO through intermolecular forces, and avoid the loss of Ti in the HTO structure, thereby resulting in a decrease in the adsorption performance for lithium ions.
[0100] Experimental Example 3
[0101] This experimental example uses sedimentary clay lithium ore in the southwest region as the test sample, and conducts the test according to the lithium ore enrichment and lithium extraction process described in Example 1. The element analysis of the lithium ore test sample is shown in the following table:
[0102] Components <![CDATA[Li2O]]> <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO Fe S <![CDATA[K2O]]> Ti MgO <![CDATA[Na2O]]> P Mn content 0.34 35.84 27.71 25.53 3.31 2.75 1.12 0.43 0.81 0.21 0.08 0.02
[0103] Figure 5 This is a process flow chart for lithium ore enrichment and lithium extraction according to Example 1 of the present invention. According to this process flow, the tailings yield, lithium grade and lithium recovery rate at each level are shown in the following table:
[0104] Grading Yield % grade% Recovery rate % Tailings 1 33.67 0.093 8.69 Tailings 2 24.69 0.173 11.84 Lithium-rich minerals 31.76 0.891 78.49 Lithium-rich materials / / 89.78
[0105] According to the data in the above table, the lithium-rich ore obtained by the lithium ore enrichment process described in Example 1 has a high Li2O enrichment ratio, which is beneficial to further reduce the recovery of lithium ions in the lithium ore. For the pickling liquid after chemical acid leaching treatment, a small part of lithium ions and other metal ions in its components can be recovered from the lithium ions in the acid solution through the separation and adsorption material prepared in Example 1, thereby improving the resource utilization of lithium ore waste liquid.
[0106] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
[0107] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a lithium separation adsorption material for enriching and extracting lithium from sedimentary clay lithium ore, characterized in that: The specific steps include: S1. Disperse diaminodiphenyl ether in NMP solvent, mix well, place in ice water bath, add 3,5-diaminobenzoic acid, add 4,4'-biphenyl ether dianhydride, stir at 300 rpm, continue stirring for 8-12 hours, add triethylamine, continue mixing for 3-5 hours, and obtain a polyamic acid solution with a solid content of 10%-15%; S2, dissolving lithium acetate in deionized water, adding CTAB and mixing evenly, dissolving tetrabutyl titanate in anhydrous ethanol, adding glacial acetic acid, placing on a magnetic stirrer and mixing evenly at a speed of 180-220 rpm, adding dropwise to the lithium acetate solution, stirring for 15-20 min at room temperature, raising the temperature to 60-70° C. and stirring until a milky white sol is generated, standing at room temperature for 24 h for aging treatment, drying at 80-100° C., and grinding to obtain an LTO precursor; S3, placing the LTO precursor prepared in step S2 in a high-temperature tube furnace, and calcining it at 700-900° C. for 3-5 hours, and obtaining LTO powder after calcination; S4, dispersing the LTO powder prepared in step S3 in a hydrochloric acid solution, raising the reaction temperature to 60-70°C, stirring the reaction at 150 rpm for 20-30 hours, filtering, washing with deionized water, and drying and grinding the HTO powder; S5, adding the HTO powder prepared in step S4 to NMP solvent, stirring and dispersing at 200-250 rpm and 25° C. for 3-5 hours, adding the polyamic acid solution prepared in step S1 after uniform dispersion, raising the temperature to 50-60° C., continuing to stir and mix for 8-10 hours, and vacuum degassing to obtain HTO / polyamic acid spinning solution; S6. The HTO / polyamic acid spinning solution prepared in step S5 is transferred to a syringe, and sent to an electrospinning machine through a needle with an inner diameter of 0.51 mm at a fixed flow rate of 2 mL / h. The voltage between the needle and the collector is controlled at 22-25 kV, and the distance between the needle and the collector is 150 mm. The spun fiber is placed in a coagulation bath solution, immersed in the coagulation bath solution for chemical imidization treatment for 12-18 hours, and then dried by supercritical CO2 to obtain a lithium extraction separation adsorption material.
2. The method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material according to claim 1, characterized in that: In step S1, the raw materials for preparing the polyamic acid solution are composed of the following weight parts: 0.45-0.6 parts of diaminodiphenyl ether, 0.05-0.15 parts of 3,5-diaminobenzoic acid, and 1 part of 4,4-biphenyl ether dianhydride; in step S1, the mass concentration of the diaminodiphenyl ether in the NMP solvent is 25-60 g / L.
3. The method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material according to claim 2, characterized in that: In step S2, the mass ratio between tetrabutyl titanate and lithium acetate is 4:1-1.
2.
4. The method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material according to claim 3, characterized in that: In step S2, the mass concentration of the lithium acetate in deionized water is 0.08-0.1 g / mL, and the added mass of the CTAB is 4%-6% of the mass of the lithium acetate.
5. The method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material according to claim 4, characterized in that: In step S2, the mass concentration of tetrabutyl titanate in anhydrous ethanol is 0.2-0.4 g / mL, and the volume ratio between glacial acetic acid and anhydrous ethanol is 2:1-1.
2.
6. The method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material according to claim 5, characterized in that: Preferably, in step S4, the mass concentration of the LTO powder in the hydrochloric acid solution is 2.5-5 g / L, and the molar concentration of hydrochloric acid in the hydrochloric acid solution is 0.1-0.2 mol / L.
7. The method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material according to claim 6, characterized in that: In step S5, the mass concentration of the HTO powder in the DMA solvent is 20-40 g / L; in step S5, the volume ratio between the HTO dispersion and the polyamic acid solution is 1:
1.
8. The method for preparing a sedimentary clay lithium ore enrichment and lithium extraction separation adsorption material according to claim 7, characterized in that: In step S6, the coagulation bath solution includes the following components in volume ratio: 2 parts of acetone, 0.1-0.2 parts of acetic anhydride, and 0.1-0.2 parts of triethylamine.
9. A material for enriching sedimentary clay lithium ore and extracting lithium separation prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The method for extracting lithium separation adsorption material to extract sedimentary clay lithium ore specifically comprises the following steps: ① Crushing sedimentary clay samples, screening and grading, and then crushing the particles of +3mm to obtain lithium ore particles with a particle size of less than 3mm; ② The lithium ore particles prepared in step ① are scrubbed so that the proportion of fine ore particles with a particle size of -0.075 mm exceeds 66.33%, and then classified to obtain classified concentrate 1 and tailings 1; ③ The classified concentrate 1 obtained in step ② is subjected to cyclone classification to obtain a classified concentrate 2 and tailings 2; ④ Sample 10 g of the graded concentrate 2 obtained in step ③ and place it in a beaker, prepare a hydrochloric acid solution with a mass concentration of 30%, add it to the graded concentrate 2, and place it on a magnetic stirrer and stir it at a speed of 200-250 rpm for 90-120 min, filter it, separate the filtrate and the precipitate, the filtrate is a lithium-containing leaching solution, wash the precipitate with deionized water until it is neutral, and dry it to obtain a lithium-rich mineral; ⑤ The lithium-containing leaching solution separated in step ④ is adjusted to pH 10-12, and the lithium extraction separation adsorption material is added and mixed, and stirred at a speed of 150 rpm in a constant temperature water bath at 25° C., and after stirring and reacting for 24 hours, filtered, and the precipitate is collected as a lithium-rich material.
Citation Information
Cited By
Novel titanium lithium adsorbent for low-salinity water body and preparation method of novel titanium lithium adsorbent
CN121178136A
Titanium-based lithium adsorbent for low salinity water body and preparation method thereof
CN121178136B