A method for preparing high-carbon high-chromium martensitic stainless steel
The method controls carbide size and distribution in high-carbon, high-chromium martensitic stainless steel through vacuum induction, consumable electrode remelting, and forging processes, addressing uneven distribution and enhancing steel performance for high-end applications.
Patent Information
- Application Number
- CN202310284473.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-03-22
AI Technical Summary
High-carbon, high-chromium martensitic stainless steel produces large and extremely unevenly distributed eutectic carbides, which are difficult to eliminate in heat treatment, affecting processing and service life.
A method involving vacuum induction and consumable electrode remelting, combined with forging pretreatment and multiple heat treatments, including upsetting, drawing, and homogenization processes, to control carbide size and distribution.
The carbides are evenly distributed and significantly reduced in size, improving the processing and service life of high-carbon martensitic stainless steel, suitable for high-end applications.
Smart Images

Figure CN116397153B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for preparing high-carbon and high-chromium martensitic stainless steel. Background Art
[0002] High-carbon, high-chromium martensitic stainless steel has the characteristics of high hardness, high wear resistance and corrosion resistance, and is widely used in bearings, piston rings and other fields. Due to the high C and Cr content in this series of steel, segregation is very easy to occur, and large pieces of eutectic carbides are inevitably produced, and the distribution is extremely uneven. It is difficult to eliminate them in the subsequent heat treatment process, which affects the processing and service life of parts. Summary of the invention
[0003] In order to overcome the defects of the above-mentioned prior art, the present invention aims at the problem that high-carbon and high-chromium martensitic stainless steel produces large and extremely unevenly distributed eutectic carbides. Through specific process parameters, the size and distribution of carbides are effectively controlled. The carbides of the high-carbon and high-chromium martensitic stainless steel produced according to the technical solution of the present invention are evenly distributed and significantly reduced in size.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing high-carbon high-chromium martensitic stainless steel, comprising the following steps:
[0005] ①Vacuum induction
[0006] Put pure iron and alloy raw materials into the crucible according to the composition ratio of 95Cr18, close the vacuum induction furnace door to evacuate, the vacuum degree is less than 1Pa, maintain the vacuum degree, turn on the power to melt and refine the alloy raw materials, obtain molten steel with designed composition, adjust the steel tapping temperature, cast the electrode rod at an overheated temperature of 80-100℃, and the baking temperature of the ingot mold is 400-600℃ to avoid electrode cracking.
[0007] ② Vacuum self-consumption
[0008] The repaired electrode rod is loaded into the crucible of a vacuum consumable furnace and the furnace body is sealed, and then the vacuum is evacuated to 0.1-0.8Pa. The vacuum degree is maintained during the smelting process. Power is turned on to generate arc discharge between the preset electrode rod and the arc starting agent at the bottom of the crucible to start remelting. The working voltage is controlled at 20.0-25.0V, the current is controlled at 4000-6000A, the consumable electrode melting rate is controlled at 2-3kg / min, and the water inlet and outlet temperatures of the crucible are 25-30°C. In the later stage of smelting, the control voltage is reduced to 15-20V, and the working current is reduced to 2000-3000A to reduce the melting rate, and solidification and shrinkage feeding are carried out in the later stage of smelting. After solidification, helium cooling is carried out to below 400°C to prepare a Φ240mm consumable steel ingot.
[0009] ③ Forging pretreatment: two upsetting, two drawing and two heat treatment processes are adopted.
[0010] ④Forging rod preparation: After heating at 1160-1200℃ and keeping warm for 2-4 hours, the steel ingot is forged into Φ50-100mm rods.
[0011] In the above technical scheme, further, the two upsetting, two drawing and two heat treatment processes described in step ③ include: the first upsetting, heating temperature 1180-1220°C, heat preservation for 1.5-2 hours, upsetting according to 50% longitudinal deformation, ensuring that the final forging temperature is greater than or equal to 950°C, using multiple forging passes, and the deformation of each pass is controlled within 10-20mm; heating the upsetting billet, heating temperature 1180-1220°C, heat preservation for 20-30 minutes, and drawing according to 100% longitudinal extension, ensuring that the final forging temperature is greater than or equal to 950°C, using multiple forging passes, and the maximum radial point deformation of each pass is controlled within 10-20mm. During the drawing process, the cross-section is first changed from a circle to an octagon, which is convenient for feeding in the length direction and avoiding too fast temperature drop at the corners, and cracking during the forging process; the first upsetting can effectively achieve the crushing of large-particle carbides. The first homogenization treatment: keep the steel ingot at 1200-1220℃ for 20-24 hours, cool it to 1050-1100℃, keep it for 8-10 hours to promote the dissolution and transformation of broken carbides.
[0012] In the above technical scheme, further, the two-upsetting, two-drawing and two-heat treatment process described in step ③ also includes: the second upsetting, heating temperature 1180-1220℃, heat preservation 1.5-2 hours, upsetting according to 50% longitudinal deformation, ensuring that the final forging temperature is greater than or equal to 950℃, using multiple forging, and the deformation of each pass is controlled at 10-20mm; heating the upsetting billet, heating temperature 1180-1220℃, heat preservation 20-30 minutes, and drawing according to 100% longitudinal extension, ensuring that the final forging temperature is greater than or equal to 950℃, using multiple forging, and the maximum radial point deformation of each pass is controlled at 10-20mm. During the drawing process, the cross section is first changed from a circle to an octagon, which is convenient for the material to be moved in the length direction, and can avoid the corner temperature drop too fast, and cracking during the forging process. The second upsetting can further promote the crushing of large-particle carbides. Second homogenization treatment: keep the steel ingot at 1200-1220℃ for 20-24 hours, cool it to 1050-1100℃, keep it for 8-10 hours, and promote the dissolution and transformation of broken carbides again.
[0013] A high-carbon, high-chromium martensitic stainless steel produced by the above method.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] The present invention solves the technical problem of large and extremely unevenly distributed eutectic carbides produced in high-carbon and high-chromium martensitic stainless steel. The carbide size and distribution are effectively controlled through specific process parameters. The carbides of the high-carbon and high-chromium martensitic stainless steel produced according to the technical solution of the present invention are evenly distributed and significantly reduced in size, thereby improving the carbide control level of high-carbon martensitic series steel grades, providing technical guarantee for expanding the market in high-end application fields of high-carbon martensitic stainless steel, and being suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a longitudinal microstructure photograph of the high carbon and high chromium martensitic stainless steel prepared in Example 1;
[0017] Figure 2 This is a transverse microstructure photograph of the high carbon and high chromium martensitic stainless steel prepared in Example 1. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available unless otherwise specified, and the quality grades are all industrial grade; the methods used are all conventional methods unless otherwise specified.
[0019] Example 1
[0020] A method for preparing high-carbon high-chromium martensitic stainless steel comprises the following steps:
[0021] 1 Vacuum induction
[0022] Pure iron and alloy raw materials are loaded into the crucible according to the composition ratio of 95Cr18. The vacuum induction furnace door is closed to evacuate the furnace. The vacuum degree is less than 1Pa. The vacuum degree is maintained and power is turned on to melt and refine the alloy raw materials to obtain molten steel with designed composition. The tapping temperature is adjusted and electrode rods are cast at an overheated 90°C. The ingot mold baking temperature is 500°C to avoid electrode cracking.
[0023] 2 Vacuum consumption
[0024] The ground electrode rod is loaded into the crucible of a vacuum consumable furnace and the furnace body is sealed, and then the vacuum is evacuated to 0.1-0.8 Pa. The vacuum degree is maintained during the smelting process, and power is turned on to generate arc discharge between the preset electrode rod and the arc starting agent at the bottom of the crucible to start remelting, the working voltage is controlled at 20.0-25.0 V, the current is controlled at 4000-6000 A, the consumable electrode melting rate is controlled at 2-3 kg / min, and the water inlet and outlet temperatures of the crucible are 25-30° C. In the later stage of smelting, the control voltage is reduced to 15-20 V, and the working current is reduced to 2000-3000 A to reduce the melting rate, and solidification and shrinkage feeding are carried out in the later stage of smelting. After solidification, helium cooling is carried out to below 400° C. to prepare a Φ240×280 mm consumable steel ingot.
[0025] 3. Forging pretreatment using two upsetting, two drawing and two heat treatment processes
[0026] 3.1 The first upsetting and drawing, heating temperature 1180 ℃, heat preservation 1.5 hours, upsetting to 140mm long, final forging temperature 980 ℃, multi-pass forging, each pass deformation 15mm. The upsetting billet is heated to 1180 ℃, heat preservation 20 minutes, lengthwise drawn to 280mm, final forging temperature 950 ℃, multi-pass forging, each pass radial deformation 15mm, the cross section is first changed from circular to octagonal during the drawing process, and then returned to circular.
[0027] 3.2 First homogenization treatment
[0028] The steel ingot was kept at 1200°C for 20 hours to promote the dissolution of carbides, and then cooled to 1050°C and kept at this temperature for 8 hours.
[0029] 3.3 The second upsetting and drawing, heating temperature 1180℃, heat preservation for 1.5 hours, upsetting to 140mm long, final forging temperature 980℃, multi-pass forging, each pass deformation 25mm. The upsetting billet is heated to 1180℃, heat preservation for 20 minutes, lengthwise drawn to 100%, final forging temperature 950℃, multi-pass forging, each pass radial deformation 25mm, the cross section is first changed from circular to octagonal during the drawing process, and then returned to circular.
[0030] 3.4 Second homogenization treatment
[0031] The steel ingot was kept at 1200°C for 20 hours to promote the dissolution of carbides, and then cooled to 1050°C and kept at this temperature for 8 hours.
[0032] 4 Forging rod preparation
[0033] After heating at 1160°C and keeping warm for 2 hours, the steel ingot is forged into a Φ50mm bar.
[0034] 5 After testing, the carbide size and distribution are effectively controlled, the size is less than 20 microns, the unevenness of eutectic carbides reaches 2-3 levels, and the longitudinal and transverse microstructure photos are as follows Figure 1 , Figure 2 shown.
[0035] Example 2
[0036] A method for preparing high-carbon high-chromium martensitic stainless steel comprises the following steps:
[0037] 1 Vacuum induction
[0038] Pure iron and alloy raw materials are loaded into the crucible according to the composition ratio of 95Cr18. The vacuum induction furnace door is closed to evacuate the furnace. The vacuum degree is less than 1Pa. The vacuum degree is maintained and power is turned on to melt and refine the alloy raw materials to obtain molten steel with designed composition. The tapping temperature is adjusted and electrode rods are cast at an overheated 90°C. The ingot mold baking temperature is 500°C to avoid electrode cracking.
[0039] 2 Vacuum consumption
[0040] The ground electrode rod is loaded into the crucible of a vacuum consumable furnace and the furnace body is sealed, and then the vacuum is evacuated to 0.1-0.8 Pa. The vacuum degree is maintained during the smelting process, and power is turned on to generate arc discharge between the preset electrode rod and the arc starting agent at the bottom of the crucible to start remelting, the working voltage is controlled at 20.0-25.0 V, the current is controlled at 4000-6000 A, the consumable electrode melting rate is controlled at 2-3 kg / min, and the water inlet and outlet temperatures of the crucible are 25-30° C. In the later stage of smelting, the control voltage is reduced to 15-20 V, and the working current is reduced to 2000-3000 A to reduce the melting rate, and solidification and shrinkage feeding are carried out in the later stage of smelting. After solidification, helium cooling is carried out to below 400° C. to prepare a Φ240×280 mm consumable steel ingot.
[0041] 3. Forging pretreatment using two upsetting, two drawing and two heat treatment processes
[0042] 3.1 The first upsetting and drawing, heating temperature 1220 ℃, heat preservation for 2.5 hours, upsetting to 140mm long, final forging temperature 960 ℃, multi-pass forging, each pass deformation 20mm. The upsetting billet is heated to 1220 ℃, heat preservation for 20 minutes, and drawn to 280mm in length direction, final forging temperature 950 ℃, multi-pass forging, each pass radial deformation 20mm, and the cross section is changed from circular to octagonal during the drawing process, and then returned to circular.
[0043] 3.2 First homogenization treatment
[0044] The steel ingot was kept at 1200°C for 20 hours to promote the dissolution of carbides, and then cooled to 1050°C and kept at this temperature for 8 hours.
[0045] 3.3 The second upsetting and drawing, the steel ingot is kept at 1220℃ for 24 hours, the carbide is promoted for 2.5 hours, upsetting to 140mm long, the final forging temperature is 980℃, multi-pass forging is adopted, and the deformation of each pass is 25mm. The upsetting billet is heated to 1180℃, kept for 20 minutes, and drawn to 100% in the length direction, the final forging temperature is 950℃, and multi-pass forging is adopted, and the radial deformation of each pass is 25mm. During the drawing process, the cross section is first changed from a circle to an octagon, and then returned to a circle.
[0046] 3.4 Second homogenization treatment
[0047] The steel ingot was kept at 1220°C for 24 hours to promote the dissolution of carbides, then cooled to 1100°C and kept at this temperature for 8 hours.
[0048] 4 Forging rod preparation
[0049] After heating at 1180°C and keeping warm for 4 hours, the steel ingot is forged into Φ80mm bar.
[0050] 5 After testing, the carbide size and distribution are effectively controlled, the size is less than 20 microns, and the eutectic carbide unevenness reaches level 2-3.
[0051] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing high carbon and high chromium martensitic stainless steel, It is characterized in that The method comprises the following steps: ① Vacuum induction: pure iron and alloy raw materials are loaded into the crucible according to the proportion of 95Cr18, the vacuum induction furnace door is closed to evacuate, the vacuum degree is less than 1 Pa, the vacuum degree is maintained, and the alloy raw materials are melted and refined to obtain molten steel with the designed composition; the steel tapping temperature is adjusted, the electrode rod is cast at an overheated temperature of 80℃-100℃, and the ingot mold baking temperature is 400℃-600℃; ② Vacuum consumable: put the electrode rods that have been repaired in step ① into the crucible of the vacuum consumable furnace and seal the furnace body, then evacuate to 0.1-0.8 Pa, maintain the vacuum degree during the smelting process, power on for remelting, the working voltage is 20.0-25.0 V, the current is 4000-6000 A, the consumable electrode melting rate is controlled at 2-3 kg / min, and the water inlet and outlet temperatures of the crucible are 25℃-30℃; in the later stage of smelting, reduce the control voltage to 15-20 V, reduce the working current to 2000-3000 A, and after solidification, cool with helium to below 400℃ to prepare a Φ240 mm consumable steel ingot; ③ Forging pretreatment: The steel ingot obtained in step ② is subjected to two upsetting, two drawing and two heat treatment processes; The two-upsetting-two-drawing-two-heat treatment process comprises: the first upsetting-drawing, heating temperature 1180°C-1220°C, heat preservation for 1.5-2 hours, upsetting according to 50% longitudinal deformation, ensuring that the final forging temperature is greater than or equal to 950°C, adopting multiple forging passes, and controlling the deformation of each pass within 10-20 mm; heating the upsetting billet, heating temperature 1180°C-1220°C, heat preservation for 20-30 minutes, drawing according to 100% longitudinal extension, ensuring that the final forging temperature is greater than or equal to 950°C, adopting multiple forging passes, and controlling the radial maximum point deformation of each pass within 10-20 mm; the first homogenization treatment: heating the steel ingot at 1200°C-1220°C, heat preservation for 20-24 hours, cooling to 1050°C-1100°C, and heat preservation for 8-10 hours; The second upsetting and drawing, heating temperature 1180 ℃ -1220 ℃, heat preservation 1.5-2 hours, upsetting according to 50% longitudinal deformation, ensuring that the final forging temperature is greater than or equal to 950 ℃, using multiple forging, each pass deformation is controlled within 10-20 mm; heating the billet after upsetting, heating temperature 1180 ℃ -1220 ℃, heat preservation for 20-30 minutes, and elongating according to 100% longitudinal extension to ensure that the final forging temperature is greater than or equal to 950 ℃, using multiple forging, each pass radial maximum point deformation is controlled within 10-20 mm; the second homogenization treatment: the steel ingot is kept at 1200 ℃ -1220 ℃ for 20-24 hours, cooled to 1050 ℃ -1100 ℃, and kept for 8-10 hours; ④Forging rod preparation: After heating at 1160℃-1200℃ and keeping warm for 2-4 hours, the steel ingot is forged into Φ50-100 mm rods.
2. A high carbon, high chromium martensitic stainless steel produced according to the method of claim 1.