A SCR catalyst for synergistic removal of CO and its preparation method and application
Through the preparation of vanadium iron tungsten oxide solid solution catalyst, combined with NH3-SCR and CO oxidation active sites, the problem of CO removal and NOx treatment in high oxygen environment is solved, efficient and stable flue gas treatment is achieved, and the cost is reduced. and waste liquid production.
Patent Information
- Application Number
- CN202310480666.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-28
AI Technical Summary
In the existing technology, it is difficult for the catalyst to effectively remove CO in a high-oxygen environment, and the preparation is complicated and costly. There are also deactivation problems, and it is impossible to achieve NH3-SCR and CO oxidation at the same time.
Using vanadium iron tungsten oxide solid solution as the catalyst, it is prepared through uniform mixing, roasting and pulverizing steps. It combines NH3-SCR and CO oxidation active sites to inhibit SO2 adsorption, enhance active site interaction and dispersion, and reduce preparation costs and waste. liquid is produced.
It achieves effective removal of CO and NOx in a high-oxygen environment, improves the activity and stability of the catalyst, simplifies the preparation process, and is suitable for mass production.
Smart Images

Figure CN116408100B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flue gas treatment, and relates to a flue gas treatment catalyst, and in particular to an SCR catalyst for synergistically removing CO, and a preparation method and application thereof. Background Art
[0002] With the development of energy and society, the demand for traditional fossil energy is increasing. However, the tail gas from industries such as coal power, steel, cement, petrochemicals, glass and incineration contains a large amount of nitrogen oxides (NOx) and CO and other pollutants, causing serious air pollution.
[0003] Among them, NOx is the main precursor of greenhouse effect, acid rain, ozone layer depletion, photochemical smog and haze, which is seriously harmful to human body. CO is a colorless, tasteless, odorless and suffocating toxic gas. CO can easily combine with hemoglobin in blood, causing people to experience dizziness, headache, nausea and other poisoning symptoms, and in severe cases, suffocation and death.
[0004] Ammonia selective catalytic reduction (NH3-SCR) is the most effective denitrification method currently in wide use. It has been maturely applied and widely promoted in thermal power, cement, steel and other industries. CO catalytic oxidation is a common method for removing CO. CO can also be used as a reducing agent to catalytically reduce NOx, and the synergistic removal of NOx and CO can be achieved without adding additional reducing agents.
[0005] However, most catalysts in the prior art have a single NH3-SCR function or a CO oxidation function, and cannot simultaneously achieve NH3-SCR denitrification and CO catalytic oxidation. Moreover, CO-SCR catalysts need to be used in an oxygen-deficient environment, while the oxygen content in industrial flue gas is mostly above 6%. Under this oxygen content, CO will undergo a strong oxidation reaction, which will make it difficult for the CO-SCR reaction to occur.
[0006] CN115069266A discloses a catalyst for simultaneously removing nitrogen oxides and carbon monoxide from flue gas, and its preparation method and application. The catalyst provided is a manganese-cobalt composite oxide or a nickel-manganese composite oxide. During preparation, the raw materials required for the constituent elements are firstly used to form a mixed solution, and then a precipitate is prepared by coprecipitation or hydrothermal reaction; the precipitate is roasted to obtain a manganese-cobalt composite oxide or a nickel-manganese composite oxide. However, the aging time required for the preparation method is relatively long, and waste liquid is inevitably generated.
[0007] CN114160186A discloses a catalyst for simultaneously removing nitrogen oxides and carbon monoxide, and its preparation method and application. The catalyst uses an acid-modified microporous or mesoporous material as a carrier, and the carrier is loaded with an active component, and the active component includes any one or a combination of at least two of copper, manganese, vanadium, cerium, niobium, cobalt or iron oxides. It can simultaneously achieve NH3-SCR and CO oxidation, but the catalyst still has the disadvantages of complex preparation and long cycle.
[0008] CN112892547A discloses a catalyst for simultaneously removing nitrogen oxides and carbon monoxide and a preparation method thereof, belonging to the field of catalyst technology. The catalyst is a supported catalyst, with γ-Al2O3 as a carrier, Mn, Cu, Ce oxides as active components, the metal salts of Mn, Cu, Ce are made into a mixed salt solution according to a certain ratio, the metal precursor is uniformly loaded on the surface of the γ-Al2O3 carrier under ultrasonic assistance conditions, and the supported catalyst is obtained after drying and roasting. However, industrial flue gas contains a certain amount of water and sulfur dioxide, which easily leads to the deactivation of the above catalyst.
[0009] Therefore, taking into account the preparation cost and use conditions of the catalyst, it is of great significance to provide an SCR catalyst for synergistic CO removal that is simple to prepare, low in cost, high in activity and good in stability, as well as a preparation method and application thereof. Summary of the invention
[0010] The object of the present invention is to provide an SCR catalyst for synergistically removing CO and a preparation method and application thereof. The preparation method uses non-precious metals as active components, which reduces the preparation cost of the catalyst. The preparation method is simple to operate and does not generate waste liquid. No additives are required during the preparation of the catalyst powder, and it is easy to produce in large quantities.
[0011] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0012] In a first aspect, the present invention provides a method for preparing an SCR catalyst for synergistically removing CO, the preparation method comprising the following steps:
[0013] (1) uniformly mixing a vanadium-containing salt, an iron-containing salt, and a tungsten-containing salt to obtain a mixture;
[0014] (2) calcining the mixture obtained in step (1) to obtain a vanadium-iron-tungsten oxide solid solution;
[0015] (3) crushing the vanadium iron tungsten oxide solid solution obtained in step (2) to obtain a crushed material;
[0016] (4) Mixing the carrier, additives, solvent and the crushed material obtained in step (3), and performing post-treatment to obtain the SCR catalyst for synergistically removing CO.
[0017] The preparation method of the present invention combines NH3-SCR, CO oxidation active sites and acid sites in the form of vanadium iron tungsten oxide solid solution, inhibits the adsorption of SO2 on the active sites, thereby reducing the poisoning of SO2 on the active sites, and accelerates the desorption of the generated CO2 from the catalyst surface; it is also beneficial for the adsorbed and activated NH3 to directly participate in the reaction on the active sites, promoting the NH3-SCR reaction; the solid solution structure can strengthen the interaction and electron transfer between different active components, and the acid sites of the catalyst isolate the active sites, so that the active sites are fully dispersed and not easy to sinter and agglomerate during the reaction process, thereby improving the activity and stability of the catalyst. Moreover, the preparation method provided by the present invention is simple to operate, does not generate waste liquid, and is suitable for mass production.
[0018] As a preferred technical solution, the uniform mixing method in step (1) includes ball milling, and the ball milling satisfies at least one of the conditions (a) to (c):
[0019] (a) the mass ratio of the grinding balls used in the ball milling to the mixed material is 8:1 to 12:1;
[0020] (b) the rotation speed of the ball mill is 250 r / min to 350 r / min;
[0021] (c) The ball milling time is 1 h to 2 h.
[0022] Ball milling can dislocate the crystal phases of vanadium-containing salts, iron-containing salts and tungsten-containing salts through mechanical shearing, increase internal defects, and make it easier to form vanadium-iron-tungsten oxide solid solutions in subsequent calcination. Then, through subsequent pulverization, while reducing the particle size of the vanadium-iron-tungsten oxide solid solution, the defect sites are increased, thereby improving the surface area and catalytic activity of the resulting SCR catalyst for synergistic CO removal.
[0023] Preferably, the mass ratio of ball milling beads to the mixed material during ball milling is 8:1 to 12:1, for example, 8:1, 9:1, 10:1, 11:1 or 12:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Exemplarily, the material of the ball milling beads includes zirconium oxide and / or agate.
[0025] Preferably, the rotation speed of the ball milling mixing is 250 r / min to 350 r / min, for example, it can be 250 r / min, 280 r / min, 300 r / min, 320 r / min or 350 r / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the ball milling mixing time is 1 h to 2 h, for example, 1 h, 1.2 h, 1.5 h, 1.6 h, 1.8 h or 2 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the molar ratio of iron to vanadium in the mixture of step (1) is 1:0.1 to 1:0.5, for example, it can be 1:0.1, 1:0.2, 1:0.3, 1:0.4 or 1:0.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] The molar ratio of iron to tungsten in the mixture of step (1) is 1:0.5 to 1:3, for example, it can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5 or 1:3, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 1:0.5 to 1:1.
[0029] Selecting a suitable molar ratio of vanadium, iron and tungsten is conducive to making the SCR catalyst for synergistic CO removal have excellent NH3-SCR and CO oxidation performance, and is conducive to making the obtained SCR catalyst for synergistic CO removal have excellent sulfur resistance. If the content of vanadium and / or iron in the mixture is small, it is not conducive to ensuring the number of active sites in the obtained catalyst; if the content of vanadium and / or iron in the mixture is large, it will cause the active sites to agglomerate, resulting in a decrease in the number of active sites, and the insufficient acid sites caused by the low relative content of tungsten will also reduce the sulfur resistance of the catalyst.
[0030] Preferably, the vanadium-containing salt in step (1) comprises any one of ammonium metavanadate, vanadium tetrachloride or vanadyl oxalate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of ammonium metavanadate and vanadium tetrachloride, a combination of vanadium tetrachloride and vanadyl oxalate, a combination of ammonium metavanadate and vanadyl oxalate, or a combination of ammonium metavanadate, vanadium tetrachloride and vanadyl oxalate.
[0031] The iron-containing salt in step (1) includes any one of ferric nitrate, ferric chloride or ferric oxalate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of ferric nitrate and ferric chloride, a combination of ferric chloride and ferric oxalate, a combination of ferric nitrate and ferric oxalate, or a combination of ferric nitrate, ferric chloride and ferric oxalate.
[0032] The tungsten-containing salt in step (1) includes any one of ammonium metatungstate, ammonium tungstate or ammonium paratungstate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of ammonium metatungstate and ammonium tungstate, a combination of ammonium tungstate and ammonium paratungstate, a combination of ammonium metatungstate and ammonium paratungstate, or a combination of ammonium metatungstate, ammonium tungstate and ammonium paratungstate.
[0033] Preferably, the calcination in step (2) satisfies at least one of conditions (d) to (g):
[0034] (d) the calcination in step (2) is carried out in an oxygen-containing atmosphere;
[0035] (e) the heating rate of the calcination in step (2) is 2°C / min to 10°C / min, for example, 2°C / min, 4°C / min, 5°C / min, 6°C / min, 8°C / min or 10°C / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0036] (f) The calcination temperature in step (2) is 500° C. to 700° C., for example, 500° C., 550° C., 600° C., 650° C. or 700° C., but is not limited to the values listed, and other values not listed within the numerical range are also applicable;
[0037] (g) The calcination time in step (2) is 2 h to 4 h, for example, 2 h, 2.5 h, 3 h, 3.5 h or 4 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] The oxygen-containing atmosphere in step (d) of the present invention comprises air.
[0039] The appropriate calcination temperature is conducive to making the obtained catalyst have good catalytic activity and excellent sulfur resistance. If the calcination temperature is too low, the mixed material cannot be completely converted into a vanadium iron tungsten oxide solid solution; if the calcination temperature is too high, the particle size of the obtained vanadium iron tungsten oxide solid solution will be too large, resulting in a decrease in the catalytic activity of the obtained catalyst. Taking into account the manufacturing cost, catalytic activity and sulfur resistance, the calcination temperature is 500°C to 700°C.
[0040] Preferably, the pulverizing method in step (3) comprises ball milling, and the ball milling satisfies at least one of conditions (h) to (j):
[0041] (h) The mass ratio of the grinding balls used in the ball mill to the vanadium iron tungsten oxide solid solution is 5:1 to 20:1, for example, 5:1, 8:1, 10:1, 12:1, 15:1, 18:1 or 20:1, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0042] (i) the rotation speed of the ball mill is 100 r / min to 500 r / min, for example, 100 r / min, 200 r / min, 300 r / min, 400 r / min or 500 r / min, but is not limited to the listed values, and other values not listed in the numerical range are also applicable;
[0043] (j) The ball milling time is 1 h to 2 h, for example, 1 h, 1.2 h, 1.5 h, 1.6 h, 1.8 h or 2 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] Exemplarily, the material of the grinding balls in step (e) includes zirconium oxide and / or agate.
[0045] Preferably, the carrier in step (4) includes one or more of anatase TiO2, SiO2, Al2O3, ZrO2, titanium tungsten silicon, and typical but non-limiting combinations include a combination of anatase TiO2 and SiO2, a combination of Al2O3 and ZrO2, a combination of SiO2, Al2O3 and ZrO2, or a combination of anatase TiO2, SiO2, Al2O3, ZrO2 and titanium tungsten silicon.
[0046] Preferably, the carrier in step (4) satisfies at least one of conditions (k) to (n):
[0047] (k) The average particle size of the carrier in step (4) is 5 μm to 10 μm, for example, 5 μm, 6 μm, 8 μm, 9 μm or 10 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0048] (l) The specific surface area of the carrier in step (4) is 30 m 2 / g to 80m 2 / g, for example, 30m 2 / g, 40m 2 / g, 50m 2 / g, 60m 2 / g, 70m 2 / g or 80m 2 / g, but not limited to the listed values, other values not listed in the numerical range are also applicable;
[0049] (m) The pore size of the carrier in step (4) ranges from 10 nm to 40 nm, for example, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm or 40 nm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0050] The pore size of the carrier of the present invention ranges from 10 nm to 40 nm. The carrier has a pore size of 30 nm under the condition that the average particle size is 5 μm to 10 μm. 2 / g to 80m 2 / g specific surface area.
[0051] (n) In step (4), the mass ratio of the carrier to the crushed material is 3:1 to 10:1, for example, 3:1, 5:1, 7:1 or 10:1, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0052] Preferably, the additive in step (4) includes any one of a release agent, a reinforcing agent, a pore former, a defoaming agent, a lubricant, a binder or a water retaining agent, or a combination of at least two thereof.
[0053] The release agent of the present invention includes but is not limited to stearic acid; the amount of the release agent used is 0.3% to 0.8% of the total mass of the carrier and the crushed material, for example, it can be 0.3%, 0.4%, 0.5%, 0.6%, 0.7% or 0.8%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] The reinforcing agent of the present invention includes but is not limited to glass fiber; the amount of the reinforcing agent used is 4% to 6% of the total mass of the carrier and the crushed material, for example, it can be 4%, 4.5%, 5%, 5.5% or 6%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0055] The pore-forming agent of the present invention includes but is not limited to pulp cotton; the usage amount of the pore-forming agent is 0.5% to 1% of the total mass of the carrier and the crushed material, for example, it can be 0.5%, 0.6%, 0.8%, 0.9% or 1%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0056] The defoaming agent of the present invention includes but is not limited to lactic acid; the usage amount of the defoaming agent is 0.8% to 1.2% of the total mass of the carrier and the crushed material, for example, it can be 0.8%, 0.9%, 1%, 1.1% or 1.2%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0057] The lubricant described in the present invention includes but is not limited to glycerol; the amount of the lubricant used is 2.5% to 3.5% of the total mass of the carrier and the crushed material, for example, it can be 2.5%, 2.7%, 3%, 3.2% or 3.5%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0058] The binder of the present invention includes but is not limited to carboxymethyl cellulose (CMC); the amount of the binder used is 0.3% to 0.5% of the total mass of the carrier and the crushed material, for example, it can be 0.3%, 0.4% or 0.5%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0059] The water retaining agent of the present invention includes but is not limited to polyethylene oxide (PEO); the usage amount of the water retaining agent is 0.8% to 1.2% of the total mass of the carrier and the crushed material, for example, it can be 0.8%, 0.9%, 1%, 1.1% or 1.2%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0060] Preferably, the post-treatment in step (4) comprises mixing, aging, extrusion, drying and calcining in sequence.
[0061] The shape of the extrusion of the present invention includes but is not limited to a honeycomb shape; the honeycomb shape is one of the shapes of the mainstream SCR catalyst. By making the extrusion shape a honeycomb shape, the present invention facilitates the use of the SCR catalyst for synergistic CO removal of the present invention to replace the mainstream catalyst.
[0062] The mixing, aging and extrusion of the post-treatment in step (4) of the present invention are carried out according to conventional methods in the art, and the present invention does not make too many limitations here.
[0063] Preferably, the mixing temperature is 20°C to 60°C, for example, 20°C, 30°C, 40°C, 50°C or 60°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0064] Preferably, the mixing time is 1 h to 3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h or 3 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0065] Preferably, the aging time is 12h to 48h, for example, it can be 12h, 15h, 18h, 20h, 24h, 28h, 30h, 35h, 36h, 40h, 45h or 48h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0066] Preferably, the drying temperature in the post-treatment is 58°C to 65°C, for example, 58°C, 60°C, 62°C, 64°C or 65°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0067] Preferably, the drying time in the post-treatment is 24 h to 36 h, for example, 24 h, 25 h, 27 h, 28 h, 30 h, 32 h, 35 h or 36 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0068] Preferably, the calcination temperature in the post-treatment is 300°C to 500°C, for example, 300°C, 350°C, 400°C, 450°C or 500°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0069] Preferably, the heating rate of calcination in the post-treatment is 2°C / min to 10°C / min, for example, it can be 2°C / min, 4°C / min, 5°C / min, 8°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0070] Preferably, the calcination time in the post-treatment is 4 h to 8 h, for example, 4 h, 5 h, 6 h, 7 h or 8 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0071] Exemplarily, the solvent in step (4) of the present invention includes aqueous ammonia and / or water;
[0072] Preferably, when the solvent is 25wt% ammonia water, the amount of the solvent used is 10% to 25% of the total mass of the carrier and the crushed material, for example, it can be 10%, 12%, 15%, 18%, 20%, 24% or 25%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0073] Preferably, when the solvent is water, the amount of the solvent used is 30% to 100% of the total mass of the carrier and the crushed material, for example, it can be 30%, 40%, 50%, 60%, 70%, 80%, 90% or 100%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0074] As a preferred technical solution of the preparation method described in the first aspect of the present invention, the preparation method comprises the following steps:
[0075] (1) uniformly mixing vanadium-containing salt, iron-containing salt and tungsten-containing salt by ball milling to obtain a mixture having a molar ratio of iron to vanadium of 1:0.1 to 1:0.5 and a molar ratio of iron to tungsten of 1:0.5 to 1:3; the mass ratio of ball milling beads to the mixture during the ball milling is 8:1 to 12:1, the speed of the ball milling is 250 r / min to 350 r / min, and the time is 1 h to 2 h;
[0076] (2) In an oxygen-containing atmosphere, the temperature is raised to 500° C. to 700° C. at a rate of 2° C. / min to 10° C. / min, and the mixed material obtained in step (1) is calcined for 2 h to 4 h to obtain a vanadium-iron-tungsten oxide solid solution;
[0077] (3) ball milling the vanadium iron tungsten oxide solid solution obtained in step (2) to obtain a crushed material; the mass ratio of the grinding balls used in the ball milling to the vanadium iron tungsten oxide solid solution is 5:1 to 20:1, the speed of the ball milling is 100 r / min to 500 r / min, and the time is 1 h to 2 h;
[0078] (4) Mixing the carrier, additives, water and the crushed material obtained in step (3), and performing mixing, aging, extrusion, drying and roasting in sequence to obtain the SCR catalyst for synergistic CO removal; the drying temperature is 58°C to 65°C, and the time is 24h to 36h; the roasting is to increase the temperature to 300°C to 500°C at a rate of 2°C / min to 10°C / min, and roast for 4h to 8h.
[0079] In a second aspect, the present invention provides an SCR catalyst for synergistic removal of CO, wherein the SCR catalyst for synergistic removal of CO is obtained by the preparation method described in the first aspect.
[0080] In a third aspect, the present invention provides an application of the SCR catalyst for synergistically removing CO as described in the second aspect, wherein the SCR catalyst for synergistically removing CO is used to remove NOx and CO from flue gas.
[0081] The source of the flue gas includes at least one of a steel sintering machine, a garbage incinerator, a biomass boiler, a solid waste blending furnace, a cement rotary kiln or an iron-extraction and zinc-reduction rotary kiln.
[0082] The application of the present invention comprises the following steps:
[0083] (I) fixing the obtained SCR catalyst for synergistic removal of CO in a gas-solid phase fixed bed reaction device;
[0084] (II) After the temperature in the gas-solid fixed bed reaction device reaches the reaction temperature, the flue gas to be treated is introduced to achieve treatment of the flue gas to be treated.
[0085] The gas-solid fixed bed reaction device in step (I) of the present invention includes not only a laboratory-level gas-solid fixed bed reaction device, but also an industrial-level gas-solid fixed bed reaction device; exemplary ones include but are not limited to SCR reactors.
[0086] Preferably, the reaction temperature in step (II) is 160°C to 360°C, for example, it can be 160°C, 180°C, 200°C, 240°C, 250°C, 280°C, 300°C, 350°C or 360°C, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 240°C to 360°C.
[0087] Preferably, the volume space velocity of the flue gas to be treated in step (II) is 3000 / h to 10000 / h, for example, 3000 / h, 5000 / h, 6000 / h, 8000 / h or 10000 / h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0088] Preferably, the NOx concentration of the flue gas to be treated in step (II) is 300 mg / m 3 Up to 800 mg / m 3 , for example, 300 mg / m 3 , 400mg / m 3 , 500mg / m 3 , 600mg / m 3 , 700mg / m 3 or 800 mg / m 3 , but not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0089] Preferably, the NH3 concentration of the flue gas to be treated in step (II) is 300 mg / m 3 Up to 800 mg / m 3 , for example, 300 mg / m 3 , 400mg / m 3 , 500mg / m 3 , 600mg / m 3 , 700mg / m 3 or 800 mg / m 3 , but not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0090] Preferably, the CO concentration of the flue gas to be treated in step (II) is 3000 mg / m 3 Up to 20000mg / m 3 , for example, 3000 mg / m 3 , 5000mg / m 3 , 6000mg / m 3 , 8000mg / m 3 , 10000mg / m 3 , 12000mg / m 3 , 15000mg / m 3 , 18000mg / m 3 or 20000mg / m 3 , but not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0091] Preferably, the SO2 concentration of the flue gas to be treated in step (II) is 0 mg / m3 Up to 500 mg / m 3 , for example, it can be 0 mg / m 3 , 100mg / m 3 , 200mg / m 3 , 300mg / m 3 , 400mg / m 3 or 500 mg / m 3 , but not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0092] Preferably, the content of H2O in the flue gas to be treated in step (II) is 0 vol% to 30 vol%, for example, it can be 0 vol%, 5 vol%, 10 vol%, 15 vol%, 20 vol%, 25 vol% or 30 vol%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0093] Preferably, the volume concentration of O2 in the flue gas to be treated in step (II) is 5% to 15%, for example, it can be 5%, 8%, 10%, 12% or 15%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0094] The NOx concentration, NH3 concentration, CO concentration, SO2 concentration, H2O content and volume concentration of O2 in the flue gas to be treated in step (II) of the present invention are independently the concentrations under standard conditions.
[0095] In the present invention, nitrogen is used as a balance gas when the flue gas to be treated is introduced in step (II).
[0096] Compared with the prior art, the present invention has the following beneficial effects:
[0097] The preparation method of the present invention combines NH3-SCR, CO oxidation active sites and acid sites in the form of vanadium iron tungsten oxide solid solution, inhibits the adsorption of SO2 on the active sites, thereby reducing the poisoning of SO2 on the active sites, and accelerates the desorption of the generated CO2 from the catalyst surface; it is also beneficial for the adsorbed and activated NH3 to directly participate in the reaction on the active sites, promoting the NH3-SCR reaction; the solid solution structure can strengthen the interaction and electron transfer between different active components, and the acid sites of the catalyst isolate the active sites, so that the active sites are fully dispersed and not easy to sinter and agglomerate during the reaction process, thereby improving the activity and stability of the catalyst. Moreover, the preparation method provided by the present invention is simple to operate, does not generate waste liquid, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0098] Figure 1 The catalyst obtained in Example 1 is 300 mg / m3 Changes of NOx conversion rate with time under SO2;
[0099] Figure 2 The catalyst obtained in Example 1 is 300 mg / m 3 How CO conversion changes with time under SO2;
[0100] Figure 3 The catalyst obtained in Example 1 was heated to 20 vol% H2O and 300 mg / m 3 Changes of NOx conversion rate with time under SO2;
[0101] Figure 4 The catalyst obtained in Example 1 was heated to 20 vol% H2O and 300 mg / m 3 CO conversion rate changes with time under SO2. DETAILED DESCRIPTION
[0102] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0103] Example 1
[0104] This embodiment provides a method for preparing an SCR catalyst for synergistically removing CO, the preparation method comprising the following steps:
[0105] (1) ball milling uniformly mixes vanadium-containing salt, iron-containing salt and tungsten-containing salt to obtain a mixture with a molar ratio of vanadium: iron: tungsten of 0.3:1:1; the mass ratio of ball milling beads to the mixture during the ball milling is 10:1, the speed of the ball milling is 300 r / min, and the time is 1.5 h; the vanadium-containing salt is ammonium metavanadate; the iron-containing salt is ferric nitrate; the tungsten-containing salt is ammonium tungstate; and the material of the ball milling beads is zirconium oxide;
[0106] (2) in an air atmosphere, heating the mixture to 600° C. at a rate of 5° C. / min, and calcining the mixture obtained in step (1) for 3 h to obtain a vanadium-iron-tungsten oxide solid solution;
[0107] (3) ball milling the vanadium iron tungsten oxide solid solution obtained in step (2) to obtain a crushed material; the mass ratio of the grinding balls used in the ball milling to the vanadium iron tungsten oxide solid solution is 10:1, the speed of the ball milling is 400 r / min, and the time is 1.5 h; the material of the grinding balls is zirconium oxide;
[0108] (4) Mixing the carrier, additives, water and the crushed material obtained in step (3), and performing mixing at 40° C. for 2 h, aging for 30 h, honeycomb extrusion, drying and calcination in sequence to obtain the SCR catalyst for synergistic CO removal; the drying temperature is 60° C. and the time is 30 h; the calcination is to increase the temperature to 400° C. at a rate of 5° C. / min and calcine for 6 h; the amount of water used is 60% of the total mass of the carrier and the crushed material.
[0109] The carrier in step (4) of this embodiment is anatase TiO2, with a pore size ranging from 10 nm to 40 nm, an average particle size of 8 μm, and a specific surface area of 64 m 2 / g; the mass ratio of the carrier to the crushed material in step (4) is 5:1.
[0110] The additives in step (4) of this embodiment include a mold release agent, stearic acid (stearic acid 1841), a reinforcing agent, glass fiber (SE4805), a pore-forming agent, commercial pulp cotton, a defoaming agent, lactic acid (chemically pure), a lubricant, glycerol (chemically pure), a binder, carboxymethyl cellulose (C0492), and a water-retaining agent, polyethylene oxide (KY170); the percentage of each additive used in the total mass of the carrier and the crushed material is: stearic acid 0.5wt%, glass fiber 5%, pulp cotton 0.8%, lactic acid 1wt%, glycerol 3wt%, carboxymethyl cellulose 0.4% and polyethylene oxide 1%.
[0111] Example 2
[0112] This embodiment provides a method for preparing an SCR catalyst for synergistically removing CO, the preparation method comprising the following steps:
[0113] (1) uniformly mixing a vanadium-containing salt, an iron-containing salt and a tungsten-containing salt by ball milling to obtain a mixture having a molar ratio of vanadium:iron:tungsten of 0.3:1:1; the mass ratio of the ball milling beads to the mixture during the ball milling is 8:1, the speed of the ball milling is 250 r / min, and the time is 2 h; the vanadium-containing salt is vanadium tetrachloride; the iron-containing salt is ferric chloride; the tungsten-containing salt is ammonium metatungstate; and the material of the ball milling beads is zirconium oxide;
[0114] (2) in an air atmosphere, heating the mixture to 600° C. at a rate of 2° C. / min, and calcining the mixture obtained in step (1) for 2 h to obtain a vanadium-iron-tungsten oxide solid solution;
[0115] (3) ball milling the vanadium iron tungsten oxide solid solution obtained in step (2) to obtain a crushed material; the mass ratio of the grinding balls used in the ball milling to the vanadium iron tungsten oxide solid solution is 5:1, the speed of the ball milling is 100 r / min, and the time is 2 h; the material of the grinding balls is zirconium oxide;
[0116] (4) Mixing the carrier, additives, water and the crushed material obtained in step (3), and performing mixing at 20° C. for 3 h, aging for 12 h, honeycomb extrusion, drying and calcination in sequence to obtain the SCR catalyst for synergistic CO removal; the drying temperature is 58° C. and the time is 36 h; the calcination is to increase the temperature to 300° C. at a rate of 2° C. / min and calcine for 8 h; the amount of water used is 30% of the total mass of the carrier and the crushed material.
[0117] The carrier in step (4) of this embodiment is anatase TiO2, with a pore size range of 10 nm to 40 nm, an average particle size of 10 μm, and a specific surface area of 32 m 2 / g; the mass ratio of the carrier to the crushed material in step (4) is 5:1.
[0118] The composition of the additives in step (4) of this embodiment is the same as that in embodiment 1; the percentage of each additive used in the total mass of the carrier and the crushed material is: stearic acid 0.3wt%, glass fiber 4%, pulp cotton 0.5%, lactic acid 0.8wt%, glycerol 2.5wt%, carboxymethyl cellulose 0.3% and polyethylene oxide 0.8%.
[0119] Example 3
[0120] This embodiment provides a method for preparing an SCR catalyst for synergistically removing CO, the preparation method comprising the following steps:
[0121] (1) ball milling uniformly mixes vanadium-containing salt, iron-containing salt and tungsten-containing salt to obtain a mixture with a molar ratio of vanadium: iron: tungsten of 0.3:1:1; the mass ratio of ball milling beads to the mixture during the ball milling is 12:1, the speed of the ball milling is 350 r / min, and the time is 1 h; the vanadium-containing salt is vanadyl oxalate; the iron-containing salt is ferric oxalate; the tungsten-containing salt is ammonium metatungstate; and the material of the ball milling beads is zirconium oxide;
[0122] (2) In an air atmosphere, the temperature is raised to 600° C. at a rate of 10° C. / min, and the mixed material obtained in step (1) is calcined for 4 hours to obtain a vanadium-iron-tungsten oxide solid solution;
[0123] (3) ball milling the vanadium iron tungsten oxide solid solution obtained in step (2) to obtain a crushed material; the mass ratio of the grinding balls used in the ball milling to the vanadium iron tungsten oxide solid solution is 20:1, the speed of the ball milling is 500 r / min, and the time is 1 hour; the material of the grinding balls is zirconium oxide;
[0124] (4) Mixing the carrier, additives, water and the crushed material obtained in step (3), and performing mixing at 60° C. for 1 hour, aging for 48 hours, honeycomb extrusion, drying and calcination in sequence to obtain the SCR catalyst for synergistic CO removal; the drying temperature is 65° C. and the time is 24 hours; the calcination is to increase the temperature to 500° C. at a rate of 10° C. / min and calcine for 4 hours; the amount of water used is 100% of the total mass of the carrier and the crushed material.
[0125] The carrier in step (4) of this embodiment is anatase TiO2, with a pore size ranging from 10 nm to 40 nm, an average particle size of 5 μm, and a specific surface area of 73 m 2 / g; the mass ratio of the carrier to the crushed material in step (4) is 5:1.
[0126] The composition of the additives in step (4) of this embodiment is the same as that in embodiment 1; the percentage of each additive used in the total mass of the carrier and the crushed material is: 0.8wt% stearic acid, 6% glass fiber, 1% pulp cotton, 1.2wt% lactic acid, 3.5wt% glycerol, 0.5% carboxymethyl cellulose and 1.2% polyethylene oxide.
[0127] In the preparation methods provided in Examples 4 to 7, except that the calcination temperature in step (2) is changed as shown in Table 1, the rest is the same as in Example 1.
[0128] Table 1
[0129] Calcination temperature (℃) Example 1 600 Example 4 500 Example 5 700 Example 6 400 Example 7 800
[0130] In the preparation methods provided in Examples 8 to 12, except that the molar ratio of vanadium: iron: tungsten in the mixture in step (1) is changed as shown in Table 2, the rest is the same as that in Example 1.
[0131] Table 2
[0132] Molar ratio of vanadium:iron:tungsten Example 1 0.3:1:1 Example 8 0.5:1:1 Example 9 0.1:1:1 Example 10 0.3:1:3 Embodiment 11 0.3:1:2 Example 12 0.3:1:0.3
[0133] Comparative Example 1
[0134] This comparative example provides a method for preparing an SCR catalyst for synergistically removing CO, and the preparation method comprises the following steps:
[0135] (1) ball milling uniformly mixes vanadium-containing salt, iron-containing salt and tungsten-containing salt to obtain a mixture with a molar ratio of vanadium: iron: tungsten of 0.3:1:1; the mass ratio of ball milling beads to the mixture during the ball milling is 10:1, the speed of the ball milling is 300 r / min, and the time is 1.5 h; the vanadium-containing salt is ammonium metavanadate; the iron-containing salt is ferric nitrate; and the tungsten-containing salt is ammonium tungstate;
[0136] (2) in an air atmosphere, heating the mixture to 600° C. at a rate of 5° C. / min, and calcining the mixture obtained in step (1) for 3 h to obtain a vanadium-iron-tungsten oxide solid solution;
[0137] (3) Mixing the carrier, additives, water and the vanadium iron tungsten oxide solid solution obtained in step (3), and performing mixing, aging, extrusion, drying and calcination in sequence to obtain the SCR catalyst for synergistic CO removal; the drying temperature is 60° C. and the time is 30 hours; the calcination is to increase the temperature to 400° C. at a rate of 5° C. / min and calcine for 6 hours.
[0138] The carrier described in step (4) of this comparative example is the same as the carrier used in Example 1.
[0139] The type and amount of the additives in step (4) of this comparative example are the same as those in Example 1.
[0140] Characterization Test
[0141] In the characterization test of the present invention, the NOx conversion rate is calculated using the following formula:
[0142] NOx conversion rate = {[(NOx) in -(NOx) out ] / (NOx) in}×100%; (NOx) in is the concentration of NOx in the flue gas at the inlet of the gas-solid fixed bed reactor; where (NOx) out is the NOx concentration in the flue gas at the outlet of the gas-solid fixed bed reactor;
[0143] In the characterization test of the present invention, the CO conversion rate is calculated using the following formula:
[0144] CO conversion rate = {[(CO) in -(CO) out ] / (CO) in}×100%; among which (CO) in is the CO concentration in the flue gas at the inlet of the gas-solid fixed bed reactor; where (CO) out It is the CO concentration in the flue gas at the outlet of the gas-solid fixed bed reactor.
[0145] I) NOx conversion rate and CO conversion rate at different reaction temperatures
[0146] Measure 30cm each 3 The catalysts provided in Examples 1 to 12 and Comparative Example 1 are respectively loaded into gas-solid fixed bed reactors, and after the temperature in the gas-solid fixed bed reactor reaches different reaction temperatures, the flue gas to be treated is introduced;
[0147] The volume space velocity of the flue gas to be treated is 5000 / h, and the NOx concentration is 500mg / m 3 , NH3 concentration is 500mg / m 3 , CO concentration is 10000mg / m 3 , the volume concentration of O2 is 10%, and N2 is the balance gas; after the reaction is stable for 1 hour, the inlet and outlet flue gases are quantitatively analyzed by a flue gas analyzer to determine the NOx conversion rate and CO conversion rate. The results are shown in Tables 3 and 4.
[0148] Table 3
[0149]
[0150]
[0151] Table 4
[0152]
[0153]
[0154] II) NOx conversion rate and CO conversion rate at different SO2 concentrations
[0155] Measure 30cm each 3 The catalysts provided in Examples 1 to 12 and Comparative Example 1 are respectively loaded into a gas-solid fixed bed reactor, and after the temperature in the gas-solid fixed bed reactor reaches the reaction temperature of 280° C., the flue gas to be treated is introduced;
[0156] The volume space velocity of the flue gas to be treated is 5000 / h, and the NOx concentration is 500mg / m 3 , NH3 concentration is 500mg / m 3 , CO concentration is 10000mg / m 3 , the volume concentration of O2 is 10%, N2 is the balance gas, and the SO2 concentration changes as shown in Table 5; after the reaction is stable for 1 hour, the inlet and outlet flue gases are quantitatively analyzed using a flue gas analyzer to determine the NOx conversion rate and CO conversion rate. The results obtained after the reaction has been running for 30 hours are shown in Table 5.
[0157] The catalyst obtained in Example 1 was 300 mg / m 3 The change of NOx with time under SO2 is as follows Figure 1 As shown; the catalyst obtained in Example 1 is 300mg / m 3 The change of CO conversion rate with time under SO2 is as follows Figure 2 shown.
[0158] Table 5
[0159]
[0160]
[0161] III) NOx conversion rate and CO conversion rate at different H2O concentrations
[0162] Measure 30cm each 3 The catalysts provided in Examples 1 to 12 and Comparative Example 1 are respectively loaded into a gas-solid fixed bed reactor, and after the temperature in the gas-solid fixed bed reactor reaches the reaction temperature of 280° C., the flue gas to be treated is introduced;
[0163] The volume space velocity of the flue gas to be treated is 5000 / h, and the NOx concentration is 500mg / m 3 , NH3 concentration is 500mg / m 3 , CO concentration is 10000mg / m 3 , the volume concentration of O2 is 10%, N2 is the balance gas, and the concentration of SO2 is 300mg / m 3 , the concentration of H2O changes as shown in Table 6; after the reaction stabilized for 1 hour, the inlet and outlet flue gases were quantitatively analyzed using a flue gas analyzer to determine the NOx conversion rate and CO conversion rate. The results obtained after the reaction ran for 30 hours are shown in Table 6.
[0164] The catalyst obtained in Example 1 was heated to 20 vol% H2O and 300 mg / m 3 The change of NOx with time under SO2 is as follows Figure 3 As shown; the catalyst obtained in Example 1 was in 20 vol% H2O and 300 mg / m 3 The change of CO conversion rate with time under SO2 is as follows Figure 4 shown.
[0165] Table 6
[0166]
[0167]
[0168] In summary, the preparation method of the present invention combines NH3-SCR, CO oxidation active sites and acid sites in the form of vanadium iron tungsten oxide solid solution, inhibits the adsorption of SO2 on the active sites, thereby reducing the poisoning of SO2 on the active sites, and accelerates the desorption of the generated CO2 from the catalyst surface; it is also beneficial for the adsorbed and activated NH3 to directly participate in the reaction on the active sites, promoting the NH3-SCR reaction; the solid solution structure can strengthen the interaction and electron transfer between different active components, and at the same time, the acid sites of the catalyst isolate the active sites, so that the active sites are fully dispersed and not easy to sinter and agglomerate during the reaction process, thereby improving the activity and stability of the catalyst. Moreover, the preparation method provided by the present invention is simple to operate, does not generate waste liquid, and is suitable for mass production.
[0169] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an SCR catalyst for synergistic removal of CO, It is characterized in that The preparation method comprises the following steps: (1) uniformly mixing a vanadium-containing salt, an iron-containing salt, and a tungsten-containing salt to obtain a mixture; (2) calcining the mixture obtained in step (1) to obtain a vanadium-iron-tungsten oxide solid solution; (3) crushing the vanadium iron tungsten oxide solid solution obtained in step (2) to obtain a crushed material; (4) mixing the carrier, additives, solvent and the crushed material obtained in step (3), and performing post-treatment to obtain the SCR catalyst for synergistic removal of CO; Wherein, the uniform mixing method in step (1) comprises ball milling mixing; The molar ratio of iron to vanadium in the mixture of step (1) is 1:0.1 to 1:0.5; The molar ratio of iron to tungsten in the mixture of step (1) is 1:0.5 to 1:3; The post-treatment in step (4) includes mixing, aging, extrusion, drying and roasting in sequence.
2. The preparation method according to claim 1, It is characterized in that The ball milling mixing satisfies at least one of the conditions (a) to (c): (a) the mass ratio of the grinding balls used in the ball milling to the mixed material is 8:1 to 12:1; (b) the rotation speed of the ball mill is 250 r / min to 350 r / min; (c) The ball milling time is 1 h to 2 h.
3. The preparation method according to claim 1, It is characterized in that The vanadium-containing salt in step (1) includes any one of ammonium metavanadate, vanadium tetrachloride or vanadyl oxalate, or a combination of at least two thereof; The iron-containing salt in step (1) includes any one of ferric nitrate, ferric chloride or ferric oxalate, or a combination of at least two thereof; The tungsten-containing salt in step (1) includes any one of ammonium metatungstate, ammonium tungstate or ammonium paratungstate, or a combination of at least two of them.
4. The preparation method according to claim 1, It is characterized in that The calcination in step (2) satisfies at least one of conditions (d) to (g): (d) the calcination in step (2) is carried out in an oxygen-containing atmosphere; (e) the heating rate of the calcination in step (2) is 2°C / min to 10°C / min; (f) the calcination temperature in step (2) is 500° C. to 700° C.; (g) The calcination time in step (2) is 2 to 4 hours.
5. The preparation method according to claim 1, It is characterized in that The pulverizing method in step (3) comprises ball milling, and the ball milling satisfies at least one of the conditions (h) to (j): (h) the mass ratio of the grinding balls used in the ball milling to the vanadium iron tungsten oxide solid solution is 5:1 to 20:1; (i) the rotation speed of the ball mill is 100 r / min to 500 r / min; (j) The ball milling time is 1 h to 2 h.
6. The preparation method according to claim 1, It is characterized in that Step (4) The carrier comprises anatase TiO 2 、Al 2 O 3 、SiO 2 、ZrO 2 Or any one of titanium, tungsten and silicon, or a combination of at least two of them.
7. The preparation method according to claim 1, It is characterized in that The carrier in step (4) satisfies at least one of the conditions (k) to (n): (k) the average particle size of the carrier in step (4) is 5 μm to 10 μm; (l) The specific surface area of the carrier in step (4) is 30 m 2 / g to 80m 2 / g; (m) the pore size of the carrier in step (4) ranges from 10 nm to 40 nm; (n) In step (4), the mass ratio of the carrier to the crushed material is 3:1 to 10:
1.
8. The preparation method according to claim 1, It is characterized in that The additives in step (4) include any one of a release agent, a reinforcing agent, a pore former, a defoaming agent, a lubricant, a binder or a water retaining agent, or a combination of at least two thereof.
9. The preparation method according to claim 1, It is characterized in that The mixing temperature is 20° C. to 60° C., and the mixing time is 1 h to 3 h.
10. The preparation method according to claim 1, It is characterized in that The aging time is 12h to 48h.
11. The preparation method according to claim 1, It is characterized in that The drying temperature in the post-treatment is 58° C. to 65° C., and the drying time is 24 h to 36 h.
12. The preparation method according to claim 1, It is characterized in that The calcination temperature in the post-treatment is at a rate of 2°C / min to 10°C / min, a temperature of 300°C to 500°C, and a time of 4h to 8h.
13. A SCR catalyst for synergistic removal of CO, It is characterized in that The SCR catalyst for synergistically removing CO is obtained by the preparation method according to any one of claims 1 to 12.
14. Use of the SCR catalyst for synergistically removing CO as claimed in claim 13, It is characterized in that The SCR catalyst for synergistically removing CO is used to remove NO in flue gas x With CO.
15. The use according to claim 14, It is characterized in that The application comprises the following steps: (I) fixing the obtained SCR catalyst for synergistic removal of CO in a gas-solid phase fixed bed reaction device; (II) After the temperature in the gas-solid fixed bed reaction device reaches the reaction temperature, the flue gas to be treated is introduced to achieve treatment of the flue gas to be treated.
16. The use according to claim 15, It is characterized in that The reaction temperature of step (II) is 160°C to 360°C.
17. The use according to claim 15, It is characterized in that The volume space velocity of the flue gas to be treated in step (II) is 3000 / h to 10000 / h.
18. The use according to claim 15, It is characterized in that The NO in the flue gas to be treated in step (II) x The concentration is 300mg / m 3 Up to 800 mg / m 3 ; NH of the flue gas to be treated in step (II) 3 The concentration is 300mg / m 3 Up to 800 mg / m 3 ; The CO concentration of the flue gas to be treated in step (II) is 3000 mg / m 3 Up to 20000mg / m 3 ; SO of the flue gas to be treated in step (II) 2 The concentration is 0mg / m 3 Up to 500 mg / m 3 ; In step (II), H 2 The content of O is 0 vol% to 30 vol%; In step (II), the O 2 The volume concentration is 5% to 15%.