A porous foam ceramic material and a preparation method thereof
By high-energy ball milling and sintering raw materials such as coal gangue to form porous foam ceramics, the problem of utilization of coal mining waste is solved, the preparation of low-density and high-pressure-resistant ceramics is realized, and the resource utilization of coal production waste is realized. Suitable for industrial production.
Patent Information
- Application Number
- CN202310279866.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-03-21
AI Technical Summary
The prior art is difficult to effectively utilize coal gangue and calcium carbonate solid waste generated during coal mining, and has not fully developed new material utilization methods.
Using the preparation method of porous foam ceramic materials, high-energy ball milling and sintering raw materials such as coal gangue, nano-alumina, binder, silica, pore-forming agent, magnesium oxide, borax and titanium oxide are used to form a porous structure. Ceramic materials use the thermal decomposition of calcium carbonate and the oxidation of straw powder to form holes, combined with the bonding effect of aluminum dihydrogen phosphate, reduce the sintering temperature and enhance the toughness of the ceramic.
The prepared porous foam ceramic has low density, low quality and high compressive strength, can withstand pressure tests of 30MPa, and realizes the resource utilization of solid waste produced by coal. The preparation method is simple and the cost is low, and it is suitable for industrial production. .
Smart Images

Figure CN116409982B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of advanced ceramic technology, and in particular to a porous foam ceramic material and a preparation method thereof. Background Art
[0002] In the process of coal mining, acidic coal wastewater and coal gangue are produced. The treatment method of acidic coal wastewater mostly adopts limestone neutralization, which will produce calcium carbonate solid waste; therefore, the disposal and resource utilization of calcium carbonate solid waste and coal gangue are also the focus of attention in the coal mining process.
[0003] In view of the above situation, it is of great significance to study how to make full use of coal gangue and calcium carbonate solid waste in the coal production process to prepare a new material. Summary of the invention
[0004] The main purpose of the present invention is to provide a porous foam ceramic material and a preparation method thereof to solve the problems in the prior art.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] In one aspect, the present invention provides a porous foam ceramic material, wherein the porous foam ceramic material is prepared by the following raw materials in parts by weight:
[0007] 30-50 parts of coal gangue, 25-42 parts of nano-alumina, 3-8 parts of binder, 5.4-8.5 parts of silicon dioxide, 10-20 parts of pore-forming agent, 1-3 parts of magnesium oxide, 0.5-1 parts of borax and 1-3 parts of titanium oxide.
[0008] Preferably, the binder is aluminum dihydrogen phosphate; and the pore-forming agent is a mixture of calcium carbonate and straw powder.
[0009] Preferably, the particle sizes of the calcium carbonate and straw powder are both less than 0.08 mm, and the ratio of the calcium carbonate to straw powder is 2 to 3: 1. The straw is the straw of crops such as rice, wheat, and corn, which is a solid waste generated by the planting industry.
[0010] In another aspect, the present invention provides a method for preparing the porous foam ceramic material according to the first aspect, comprising the following steps:
[0011] (1) placing the coal gangue in a crusher to crush it into coal gangue particles;
[0012] (2) placing the gangue particles in step (1) into a high-energy ball mill for ball milling to obtain gangue powder;
[0013] (3) adding nano-alumina, a binder, silicon dioxide, a pore-forming agent, magnesium oxide, borax and titanium oxide to the gangue powder in step (2), and placing the mixture in a planetary ball mill for ball milling to obtain powder A;
[0014] (4) placing the powder A in step (3) into a tablet press to form a ceramic raw sheet;
[0015] (5) placing the ceramic raw sheet in step (4) into a muffle furnace for high-temperature sintering, and after roasting and heat preservation, cooling to room temperature with the furnace to obtain a porous foam ceramic.
[0016] The coal gangue, a waste from coal production, was analyzed by X-ray fluorescence spectrometry technology, and its elemental composition was found to be carbon, SiO2, Al2O3, CaO, Fe2O3, etc., and its material composition was kaolin and quartz; as a raw material for the production of porous foam ceramics, it not only realizes the utilization of waste, but also provides a material basis for the preparation of porous foam ceramics.
[0017] Calcium carbonate is a solid waste generated during the treatment of acidic coal wastewater produced during coal mining. When the ceramic raw sheet is sintered at high temperature, calcium carbonate is decomposed by heat to produce gas, which creates pores inside the ceramic; the main components of straw powder are crude fiber and carbohydrates, which are oxidized to produce carbon dioxide during high-temperature sintering, which creates pores inside the ceramic; thus, the characteristic of solid waste calcium carbonate to produce carbon dioxide at high temperature is used to make porous ceramics. During the sintering process, the combustion of carbon in coal gangue, the combustion of straw powder and the thermal decomposition of calcium carbonate produce gas pores, which make the ceramic have a porous structure after sintering.
[0018]
[0019] Aluminum dihydrogen phosphate is used as a binder in the preparation of porous foam ceramic materials. When added with aluminum dihydrogen phosphate, it will dehydrate to form aluminum polyphosphate during high-temperature sintering, and then form polyphosphate glass to bond the high-temperature oxide particles. The polyphosphate glass relies on its internal bond energy to enhance the toughness and compressive strength of the ceramic. Moreover, when aluminum dihydrogen phosphate decomposes during high-temperature sintering, it will only release water vapor without producing toxic or harmful substances.
[0020] In addition, magnesium oxide, borax, and titanium oxide will form a solid solution with silicon dioxide and aluminum oxide at high temperatures, lowering the softening temperature of silicon dioxide and aluminum oxide, and lowering the sintering temperature of ceramics, allowing the ceramics to form a ceramic phase under medium temperature conditions.
[0021] Preferably, the particle size of the coal gangue particles in step (1) is less than 1 mm.
[0022] Preferably, the rotation speed of the high-energy ball mill in step (2) is 600-900 r / min, and the ball milling time is 60-180 min; and the particle size of the coal gangue powder is less than 0.075 mm.
[0023] Preferably, the rotation speed of the planetary ball mill in step (3) is 500-800 r / min, and the ball milling time is 200-500 min.
[0024] Preferably, the calcination temperature in step (5) is 1100-1200° C., and the holding time is 4-8 hours.
[0025] The beneficial effects of the present invention are:
[0026] 1. The porous foam ceramic prepared by the present invention has the characteristics of low density, low mass and high compressive strength, and can withstand a pressure test of 30 MPa.
[0027] 2. The raw materials of coal gangue and calcium carbonate used in the present invention are all from solid waste generated during coal production, thus realizing resource utilization of solid waste from coal production.
[0028] 3. The preparation method of the porous foam ceramic material of the present invention is not only simple but also low in cost and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A cross-sectional view of a porous foam ceramic material prepared in Example 1 of the present invention;
[0030] Figure 2 A cross-sectional view of a porous foam ceramic material prepared in Example 2 of the present invention;
[0031] Figure 3 This is a microscopic morphology of the porous foam ceramic material prepared in Example 3 of the present invention;
[0032] Figure 4 A cross-sectional view of a porous foam ceramic material prepared in Example 4 of the present invention;
[0033] Figure 5 This is a cross-sectional view of a porous foam ceramic material prepared in Example 5 of the present invention; DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0035] The terms "first", "second" and "third" in this application are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second" and "third" can explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. All directional indications in the embodiments of the present application (such as up, down, left, right, front, back...) are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.
[0036] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0037] Example 1
[0038] The porous foam ceramic material of this embodiment is prepared by the following raw materials in parts by weight: 30 parts of coal gangue, 25 parts of nano-alumina, 3 parts of aluminum dihydrogen phosphate, 5.4 parts of silicon dioxide, 10 parts of pore formers, 1 part of magnesium oxide, 0.5 parts of borax, and 1 part of titanium oxide. The pore former is a mixture of calcium carbonate and straw powder in a ratio of 2:1.
[0039] Preparation method of porous foam ceramic material:
[0040] 1.1 Treatment of coal gangue
[0041] (1) The coal gangue is placed in a crusher and crushed into particles with a size less than 1 mm.
[0042] (2) The coal gangue particles were placed in a high-energy ball mill at a rotation speed of 600 r / min for 180 min, and the coal gangue powder with a particle size less than 0.075 mm was sieved using a 200-mesh sieve.
[0043] 1.2 Preparation of porous foam ceramics:
[0044] (1) Coal gangue powder, nano-alumina, aluminum dihydrogen phosphate, silicon dioxide, calcium carbonate, straw powder, magnesium oxide, borax and titanium oxide are weighed according to the above weight ratio.
[0045] (2) The above materials were placed in a planetary ball mill at a rotation speed of 500 r / min and ball-milled for 500 min to obtain powder A.
[0046] (3) Powder A is placed in a tablet press and pressed into ceramic tablets.
[0047] (4) The ceramic raw sheet is placed in a muffle furnace for high-temperature sintering, kept at 1100°C for 4 hours, and cooled to room temperature to obtain a porous foam ceramic material.
[0048] The cross-section of porous foam ceramic material is shown in Figure 1 As shown by Figure 1 It can be seen that after the sample was kept at 1100°C for 4 hours and then surface polished, the surface showed porosity. These pores reduced the volume density of the foam ceramic. The porosity of the ceramic serves as the basic condition for ceramic thermal insulation.
[0049] The porous foam ceramic material is subjected to pressure testing. The upper and lower surfaces of the sintered ceramic are polished and parallel, and then placed on a pressure testing machine for pressure testing. The size of the ceramic is input into the system. After applying pressure, the system will calculate the compressive strength of the ceramic based on the size of the ceramic and the load pressure. The compressive strength of the ceramic prepared in Example 1 is 32.3 Mpa.
[0050] Example 2
[0051] The porous foam ceramic material of this embodiment is prepared by the following raw materials in parts by weight: 35 parts of coal gangue, 30 parts of nano-alumina, 4 parts of aluminum dihydrogen phosphate, 5.7 parts of silicon dioxide, 12 parts of pore formers, 1.2 parts of magnesium oxide, 0.6 parts of borax, and 1.3 parts of titanium oxide. The pore former is a mixture of calcium carbonate and straw powder in a ratio of 3:1.
[0052] Preparation method of porous foam ceramic material:
[0053] 2.1 Treatment of coal gangue
[0054] (1) The coal gangue is placed in a crusher and crushed into particles with a size less than 1 mm.
[0055] (2) The coal gangue particles were placed in a high-energy ball mill at a rotation speed of 700 r / min for 160 min, and the coal gangue powder with a particle size less than 0.075 mm was sieved using a 200-mesh sieve.
[0056] 2.2 Preparation of porous foam ceramics:
[0057] (1) Coal gangue powder, nano-alumina, aluminum dihydrogen phosphate, silicon dioxide, calcium carbonate, straw powder, magnesium oxide, borax and titanium oxide are weighed according to the above weight ratio.
[0058] (2) The above materials were placed in a planetary ball mill at a rotation speed of 600 r / min and ball-milled for 450 min to obtain powder A.
[0059] (3) Powder A is placed in a tablet press and pressed into ceramic tablets.
[0060] (4) The ceramic raw sheet is placed in a muffle furnace for high-temperature sintering, kept at 1100°C for 6 hours, and cooled to room temperature to obtain a porous foam ceramic material.
[0061] The cross-section of porous foam ceramic material is shown in Figure 2 As shown by Figure 2 It can be seen that after the sample was kept at 1100°C for 6 hours and then surface polished, the surface showed porosity. These pores reduced the volume density of the foam ceramic. The porosity of the ceramic serves as the basic condition for ceramic thermal insulation.
[0062] The porous foam ceramic material is subjected to pressure test: the upper and lower surfaces of the sintered ceramic are polished and parallel, and then placed on a pressure tester for pressure test. The size of the ceramic is input into the system. After applying pressure, the system will calculate the compressive strength of the ceramic according to the size of the ceramic and the load pressure. The compressive strength of the ceramic prepared in Example 2 is 34.6Mpa.
[0063] Example 3
[0064] The porous foam ceramic material of this embodiment is prepared by the following raw materials in parts by weight: 40 parts of coal gangue, 35 parts of nano-alumina, 5 parts of aluminum dihydrogen phosphate, 6 parts of silicon dioxide, 15 parts of pore former, 2 parts of magnesium oxide, 0.7 parts of borax, and 2 parts of titanium oxide. The pore former is a mixture of calcium carbonate and straw powder in a ratio of 2.5:1.
[0065] Preparation method of porous foam ceramic material:
[0066] 3.1 Treatment of coal gangue
[0067] (1) The coal gangue is placed in a crusher and crushed into particles with a size less than 1 mm.
[0068] (2) The coal gangue particles were placed in a high-energy ball mill at a rotation speed of 800 r / min for 120 min, and the coal gangue powder with a particle size less than 0.075 mm was sieved using a 200-mesh sieve.
[0069] 3.2 Preparation of porous foam ceramics:
[0070] (1) Coal gangue powder, nano-alumina, aluminum dihydrogen phosphate, silicon dioxide, calcium carbonate, straw powder, magnesium oxide, borax and titanium oxide are weighed according to the above weight ratio.
[0071] (2) The above materials were placed in a planetary ball mill at a rotation speed of 700 r / min and ball-milled for 300 min to obtain powder A.
[0072] (3) Powder A is placed in a tablet press and pressed into ceramic tablets.
[0073] (4) The ceramic raw sheet is placed in a muffle furnace for high-temperature sintering, kept at 1200°C for 4 hours, and cooled to room temperature to obtain a porous foam ceramic material.
[0074] The cross-section of porous foam ceramic material is shown in Figure 3 As shown by Figure 3 It can be seen that the microscopic morphology of the sample after surface grinding under a scanning electron microscope after being kept at 1200°C for 4 hours shows that the surface is porous. These pores reduce the volume density of the foam ceramic. The porosity of the ceramic serves as the basic condition for ceramic thermal insulation.
[0075] The porous foam ceramic material is subjected to pressure test: the upper and lower surfaces of the sintered ceramic are polished and parallel, and then placed on a pressure tester for pressure test. The size of the ceramic is input into the system. After applying pressure, the system will calculate the compressive strength of the ceramic according to the size of the ceramic and the load pressure. The compressive strength of the ceramic prepared in Example 3 is 34.4Mpa.
[0076] Example 4
[0077] The porous foam ceramic material of this embodiment is prepared by the following raw materials in parts by weight: 45 parts of coal gangue, 35 parts of nano-alumina, 7 parts of aluminum dihydrogen phosphate, 7.5 parts of silicon dioxide, 17 parts of pore former, 2.5 parts of magnesium oxide, 0.8 parts of borax, and 2.5 parts of titanium oxide. The pore former is a mixture of calcium carbonate and straw powder in a ratio of 2:1.
[0078] Preparation method of porous foam ceramic material:
[0079] 4.1 Treatment of coal gangue
[0080] (1) The coal gangue is placed in a crusher and crushed into particles with a size less than 1 mm.
[0081] (2) The coal gangue particles were placed in a high-energy ball mill at a rotation speed of 900 r / min for 60 min, and the coal gangue powder with a particle size less than 0.075 mm was sieved using a 200-mesh sieve.
[0082] 4.2 Preparation of porous foam ceramics:
[0083] (1) Coal gangue powder, nano-alumina, aluminum dihydrogen phosphate, silicon dioxide, calcium carbonate, straw powder, magnesium oxide, borax and titanium oxide are weighed according to the above weight ratio.
[0084] (2) The above materials were placed in a planetary ball mill at a rotation speed of 800 r / min and ball-milled for 200 min to obtain powder A.
[0085] (3) Powder A is placed in a tablet press and pressed into ceramic tablets.
[0086] (4) The ceramic raw sheet is placed in a muffle furnace for high-temperature sintering, kept at 1200°C for 6 hours, and cooled to room temperature to obtain a porous foam ceramic material.
[0087] The morphology of porous foam ceramic materials is shown in Figure 4 As shown by Figure 4 It can be seen that after the sample was kept at 1200℃ for 6 hours and then surface polished, the microscopic morphology under a scanning electron microscope shows mullite whiskers. Mullite has good heat resistance and heat corrosion resistance.
[0088] The porous foam ceramic material is subjected to pressure test: the upper and lower surfaces of the sintered ceramic are polished and parallel, and then placed on a pressure tester for pressure test. The size of the ceramic is input into the system. After applying pressure, the system will calculate the compressive strength of the ceramic according to the size of the ceramic and the load pressure. The compressive strength of the ceramic prepared in Example 4 is 35.1 Mpa.
[0089] Example 5
[0090] The porous foam ceramic material of this embodiment is prepared by the following raw materials in parts by weight: 50 parts of coal gangue, 42 parts of nano-alumina, 8 parts of aluminum dihydrogen phosphate, 8.5 parts of silicon dioxide, 20 parts of pore former, 3 parts of magnesium oxide, 1 part of borax, and 3 parts of titanium oxide. The pore former is a mixture of calcium carbonate and straw powder in a ratio of 2:1.
[0091] Preparation method of porous foam ceramic material:
[0092] 5.1 Treatment of coal gangue
[0093] (1) The coal gangue is placed in a crusher and crushed into particles with a size less than 1 mm.
[0094] (2) The gangue particles were placed in a high-energy ball mill at a rotation speed of 800 r / min and ball-milled for 100 min. A 200-mesh sieve was used to sieve out the gangue powder with a particle size less than 0.075 mm.
[0095] 5.2 Preparation of porous foam ceramics:
[0096] (1) Coal gangue powder, nano-alumina, aluminum dihydrogen phosphate, silicon dioxide, calcium carbonate, straw powder, magnesium oxide, borax and titanium oxide are weighed according to the above weight ratio.
[0097] (2) The above materials were placed in a planetary ball mill at a rotation speed of 700 r / min and ball-milled for 400 min to obtain powder A.
[0098] (3) Powder A is placed in a tablet press and pressed into ceramic tablets.
[0099] (4) The ceramic raw sheet is placed in a muffle furnace for high-temperature sintering, kept at 1150° C. for 5 hours, and cooled to room temperature to obtain a porous foam ceramic material.
[0100] The cross-section of porous foam ceramic material is shown in Figure 5 As shown by Figure 5 It can be seen that after the sample was kept at 1150°C for 5 hours and then surface polished, the surface showed porosity. These pores reduced the volume density of the foam ceramic. The porosity of the ceramic serves as the basic condition for ceramic thermal insulation.
[0101] The porous foam ceramic material is subjected to pressure testing: the upper and lower surfaces of the sintered ceramic are polished and parallel, and then placed on a pressure testing machine for pressure testing. The size of the ceramic is input into the system. After applying pressure, the system will calculate the compressive strength of the ceramic based on the size of the ceramic and the load pressure. The compressive strength of the ceramic prepared in Example 5 is 32.4 Mpa.
[0102] Comparative Example 1
[0103] 30 parts of coal gangue, 30 parts of nano-alumina, 3 parts of binder, and 0.5 parts of borax were mixed, and the preparation method was the same as the ceramic preparation process described in Example 1, and the mixture was kept at 1100°C for 4 hours, and then cooled to room temperature with the furnace to obtain a ceramic material. The compressive strength test was performed on the ceramic, and the compressive strength of the ceramic was 20.6Mpa.
[0104] In summary, the porous foam ceramics prepared by the present invention have the characteristics of low density, low mass and high compressive strength, can enhance the compressive strength of the porous foam ceramics, and can withstand a pressure test of 30MPa, and can be used as a heat insulation board for a furnace. At the same time, the raw materials used to prepare the porous foam ceramic material come from the solid waste coal gangue and calcium carbonate generated during coal production, realizing the resource utilization of solid waste from coal production. And the preparation method of the porous foam ceramic material is not only simple, but also low in cost, and is suitable for industrial production.
[0105] The specific implementation methods of the invention are described in detail above, but they are only examples, and the invention is not limited to the specific implementation methods described above. For those skilled in the art, any equivalent modification or substitution of the invention is also within the scope of the invention, therefore, the equalization, modification, improvement, etc. made without departing from the spirit and principle of the invention should be included in the scope of the invention.
Claims
1. A porous foam ceramic material, It is characterized in that The porous foam ceramic material is prepared by including the following raw materials in parts by weight: 30-50 parts of coal gangue, 25-42 parts of nano-alumina, 3-8 parts of binder, 5.4-8.5 parts of silicon dioxide, 10-20 parts of pore-forming agent, 1-3 parts of magnesium oxide, 0.5-1 parts of borax, and 1-3 parts of titanium oxide; The binder is aluminum dihydrogen phosphate; the pore-forming agent is a mixture of calcium carbonate and straw powder; The particle size of the calcium carbonate and straw powder is less than 0.08mm, the ratio of calcium carbonate and straw powder is 2 to 3: 1; The calcium carbonate is solid waste obtained by legally treating coal acid wastewater in limestone; The method for preparing the porous foam ceramic material comprises the following steps: (1) placing the coal gangue in a crusher to crush it into coal gangue particles; (2) placing the gangue particles in step (1) into a high-energy ball mill for ball milling to obtain gangue powder; (3) adding nano-alumina, a binder, silicon dioxide, a pore-forming agent, magnesium oxide, borax and titanium oxide to the gangue powder in step (2), and placing the mixture in a planetary ball mill for ball milling to obtain powder A; (4) placing the powder A in step (3) into a tablet press and pressing it into a ceramic raw tablet; (5) placing the ceramic raw sheet in step (4) into a muffle furnace for high-temperature sintering, and after roasting and heat preservation, cooling to room temperature with the furnace to obtain a porous foam ceramic; The calcination temperature in step (5) is 1100-1200° C., and the holding time is 4-8 hours.
2. The porous foam ceramic material according to claim 1, It is characterized in that The particle size of the coal gangue particles in step (1) is less than 1 mm.
3. The porous foam ceramic material according to claim 1, It is characterized in that The rotation speed of the high-energy ball mill in step (2) is 600-900 r / min, and the ball milling time is 60-180 min; the particle size of the coal gangue powder is less than 0.075 mm.
4. The porous foam ceramic material according to claim 1, It is characterized in that The rotation speed of the planetary ball mill in step (3) is 500-800 r / min, and the ball milling time is 200-500 min.