A kind of low peel strength fluorine release film and preparation method thereof

By using the combination of FKM and PVC composite resin layers, PET substrate layer and reinforcement layer in the release film, combined with corona treatment technology, the problems of easy loss and low production efficiency of the existing release film are solved, and the low production efficiency of the existing release film is achieved Peel strength and flat surfaces meet the demands of the electronics and fuel cell industries and reduce production costs.

CN116410502BActive Publication Date: 2024-12-03SHANDONG DONGYUE POLYMER MATERIAL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111671634.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-12-03
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

The existing release films are prone to scratch loss and fall off during storage, transportation and use, which affects product performance, and take a long time to process in large-scale production, and the bonding strength between the substrate layer and the graft layer is poor and the cost is high.

Method used

The composite resin layer is composed of FKM and PVC, combined with the PET substrate layer and the reinforcement layer, and the bond fastness is improved through the corona treatment system, and the composite resin layer is coated with a perfluorosulfonic acid resin film to control the peel strength. 20-50mN/cm, reduce costs.

Benefits of technology

It achieves low peel strength, smooth and smooth film surface, suitable for continuous production, reduces production costs, improves high temperature resistance, corrosion resistance and wear resistance, and meets the needs of the electronics industry and fuel cell industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003453172320000011
    Figure HDA0003453172320000011
Patent Text Reader

Abstract

The invention discloses a low peel strength fluorine release film and a preparation method thereof. The low peel strength fluorine release film comprises a PET substrate layer, a reinforcement layer and a compound resin layer. The substrate layer is PET; the reinforcement layer is formed by modifying the PET substrate layer by inputting high-energy ions in a corona treatment system, and is arranged above the PET substrate layer; the compound resin layer is a FKM-PVC blend, which is coated on the reinforcement layer, and the firmness of the compound resin layer and the reinforcement layer is 5B. The perfluorosulfonic acid resin film can be attached to the compound resin layer, and there is no corrosion on the surface, and the peel strength is 20-50mN / cm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fluorine release films, and in particular relates to a low peel strength fluorine release film and a preparation method thereof. Background Art

[0002] At present, the consumption of high-tech products is huge, and the electronics industry is developing rapidly. Among them, there is a huge demand for flexible circuit boards, which requires a large amount of release films. At the same time, with the rise of the fuel cell vehicle industry, its fuel cell preparation process also requires a large amount of release films. Currently on the market, release films are mostly silicone oil films and fluorine films, such as PET silicone oil films and PET fluorine films. This type of release film is easy to scratch and lose, fall off, and easily cause product contamination and affect product performance during storage, transportation and use, and cannot meet the needs. The development of fluorine-containing functional PET release film products can meet the needs of the growing electronics industry, automobile industry and emerging fuel cell industry, and has commercial development value and broad market prospects.

[0003] Patent CN209447937U discloses a backing film for a perfluorinated proton exchange membrane, including a substrate layer, an activation layer, and a graft layer, which has the advantages of heat resistance, solvent resistance, and corrosion resistance. However, this method may have the following problems: 1. The processing time is long, which is not conducive to large-scale production. 2. The substrate layer and the graft layer have poor bonding strength, and a stable composite material cannot be obtained.

[0004] Patent CN210203836U discloses a fluorine release film, including a substrate layer, a corona layer and a fluorosilicone release layer. The fluorosilicone release and residual adhesion can reach more than 90%, and it is easy to process, but the cost is relatively high. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the present invention provides a low peel strength fluorine release film, the composite resin layer of the release film and the polyester film (PET) substrate layer are firmly bonded to meet the requirements of continuous production of the release film, and the release film has the characteristics of being easy to peel and having a smooth film surface.

[0006] The low peel strength fluorine release film comprises a base layer and a compound resin layer.

[0007] The composite resin layer includes FKM (fluororubber) and PVC (polyvinyl chloride). Fluorine has the largest electronegativity, a lower atomic polarizability (0.557), and a smaller atomic radius (0.13nm), which makes the CF bond have a shorter bond length, higher bond energy, and lower surface free energy. Since fluorocarbon polymers are not easy to react with oxygen, FKM has good oxygen resistance and chemical stability; at the same time, the CF bond has a good shielding effect on the main chain of organic matter, making it have better stability. However, FKM also has the defects of poor wear resistance, poor processing performance, and high price. Therefore, the use of FKM in combination with PVC can improve its addition performance and reduce costs.

[0008] The mass ratio of the above-mentioned FKM and PVC compound is (0.6-1):1.2. The above-mentioned mass ratio can ensure that the cost is reduced while maintaining a low peel strength. Ordinary plastic materials such as polyester, polyvinyl chloride, polyethylene, etc. have a large peeling force with perfluorosulfonic acid resin film, and have a higher adhesive peeling force value than that allowed by pressure-sensitive adhesive peeling film. For FKM material, because the fluorine atoms in its molecular chain have a strong electronegativity, the fluorine nucleus has a strong binding effect on the extranuclear electrons and bonding electron clouds, and the covalent bond between carbon atoms and fluorine atoms has low polarizability, which makes the FKM material have extremely low surface free energy, so its interaction with the perfluorosulfonic acid resin film is low, and the peeling strength is low.

[0009] Furthermore, the thickness of the composite resin layer is 90-300 nm.

[0010] The base layer comprises a PET base layer and a reinforcement layer.

[0011] Furthermore, the compound resin layer, the reinforcement layer and the PET substrate layer are arranged in sequence from top to bottom.

[0012] The thickness of the PET substrate layer is 50-150 μm.

[0013] The reinforcing layer is formed by modifying the PET substrate layer by inputting high-energy particles through a corona treatment system, so as to improve the bonding strength between the compound resin layer and the PET substrate layer.

[0014] Furthermore, the thickness of the reinforcement layer is 50-100 nm. When the thickness exceeds the standard, the firmness of the reinforcement layer and the composite resin layer will be reduced; when the thickness is too low, the price of the reinforcement layer is high, resulting in increased costs.

[0015] Furthermore, the firmness of the reinforcing layer and the compound resin layer is 5B, where 5B means that the amount of peeling between the reinforcing layer and the compound resin layer is 0%.

[0016] The composite resin layer may be laminated with a perfluorosulfonic acid resin film.

[0017] Furthermore, after the perfluorosulfonic acid resin film is coated on the surface of the composite resin layer, there is no corrosion phenomenon, and the peel strength is 20-50mN / cm.

[0018] The present invention also provides a method for preparing the above-mentioned low peel strength fluorine release film:

[0019] (1) Preparation of reinforcing layer: The PET substrate layer is modified by inputting high-energy ions using a corona treatment system to form a polar reinforcing layer to improve the bonding strength between the compound resin layer and the PET substrate layer.

[0020] (2) Dissolution of FKM and PVC: FKM and PVC should be dissolved separately. FKM is dissolved at 40-60°C. During the dissolution process, dioctyl phthalate (DOP) is added to obtain FKM solution. PVC is dissolved at room temperature to obtain PVC solution. After dissolution, they are stored separately. Two hours before coating, the two solutions are mixed in proportion, diisopropylbenzene peroxide (DCP) is added as a compatibilizer and stirred evenly to obtain solution A.

[0021] (3) Curing treatment: Solution A is coated on the reinforcing layer and then cured.

[0022] The energy density of the corona treatment in step (1) is 120-160W·min / ㎡. When the energy density is less than 120W·min / ㎡, the reinforcing layer cannot completely cover the PET substrate, resulting in leakage points in the reinforcing layer; when the energy density is greater than 160W·min / ㎡, the PET substrate begins to deform, and the greater the energy density, the more severe the deformation of the PET substrate until it is punctured. The energy density used by the corona treatment system is best when it is 120-160W·min / ㎡, which ensures that the reinforcing layer completely covers the PET substrate layer without causing the PET substrate to begin to deform.

[0023] In step (2), the amount of PVC is 80-100phr, the amount of FKM is 48-84phr, the amount of DCP is 1-4phr, and the amount of DOP is 5-10phr; the solvent of the FKM and PVC solution is THF, and the concentration of the FKM solution is 0.023g / ml-0.046g / ml; the solid content of the solution A is 1-6%, and the viscosity is 2.27-5.81MPa·S. The above-mentioned DOP is added during the melting process of FKM, mainly to soften the FKM. Under the action of the DOP softener and the DCP compatibilizer, PVC is added to the FKM for blending. The two have good compatibility and high cross-linking density, which can improve the corrosion resistance of FKM, so that the corrosion resistance of this product is enhanced compared with other types of release films.

[0024] The curing temperature in step (3) is 120° C. and the curing time is 60 seconds.

[0025] Beneficial Effects

[0026] 1. The FKM-PVC blend of the composite resin layer provided by the present invention is compounded at a certain ratio, and the FKM interacts with the PVC, so that the internal structure of the composite resin layer is very stable, thereby having good high temperature resistance, and the surface of the composite resin layer has a very dense surface structure, so that the surface of the film is smooth and clean; and the FKM material has extremely low surface free energy, and the force between it and the perfluorosulfonic acid resin film is low, and the peel strength is 20-50mN / cm.

[0027] 2. Under the action of DCP compatibilizer and DOP softener, PVC is added to FKM for blending. The two have good compatibility and high cross-linking density, which can improve the wear resistance and high humidity resistance of FKM and reduce product costs.

[0028] 3. PET as the base material layer has the advantages of wide sources, good mechanical properties, good thermal stability, high transparency, sufficient supply and low price, which can meet the continuous production requirements of fluorine release film.

[0029] 4. After the PET substrate layer is treated by the corona treatment system, a reinforcement layer is formed on the PET substrate layer, so that the surface of the substrate layer changes from a smooth surface to a rough surface, so as to enhance the firmness between the compound resin layer and the PET substrate layer.

[0030] 5. The processing time of the compounded resin layer is short, which is conducive to large-scale production, and the perfluorosulfonic acid resin film does not corrode, which verifies that the present invention can be used as a release film for the perfluorosulfonic acid resin film. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of the cross-sectional structure of a low peel strength fluorine release film with a perfluorosulfonic acid resin film attached to the surface. DETAILED DESCRIPTION

[0032] The products used in the following implementation methods are all commercially available products, PVC is a product of Dongyue Chemical Co., Ltd., model G5; FKM is a product of DuPont, model G-911; DCP is of Aladdin analytical grade; and DOP is of Aladdin analytical grade.

[0033] Embodiment 1:

[0034] The fluorine release film of the present invention is described in Figure 1 , including a PET substrate layer, a reinforcement layer and a compound resin layer, wherein the compound resin layer, the reinforcement layer and the PET substrate layer are arranged in sequence from top to bottom.

[0035] The thickness of the PET substrate layer was 75 μm.

[0036] The reinforcing layer is formed by modifying the PET substrate layer by inputting high-energy ions through a corona treatment system, and is arranged on top of the PET substrate layer. The energy density of the corona treatment is 140W·min / ㎡, and the thickness of the reinforcing layer is 80nm.

[0037] The compound resin layer is obtained by compounding FKM and PVC. 3g of FKM is dissolved in 130ml THF at 50°C, and 0.076g of DOP is added during the dissolution process to obtain a FKM solution; 4.6g of PVC is dissolved at room temperature to obtain a PVC solution. Two hours before coating, the above FKM solution and PVC solution are mixed and stirred at a ratio of FKM:PVC=1:1.2, and then 0.76g of DCP is added to obtain solution A. The solid content of the solution A is 5%. The above solution A is coated on the reinforcing layer and cured at 120°C for 60s to obtain a compound resin layer. The thickness of the compound resin layer is 100nm.

[0038] According to the ASTM-D3359 standard test, the firmness of the compound resin layer and the reinforcement layer is 5B, and the compound resin layer does not fall off from the reinforcement layer. A perfluorosulfonic acid resin film is coated on the compound resin layer, and the perfluorosulfonic acid resin film is not damaged, and its peel strength is 30mN / cm.

[0039] Embodiment 2:

[0040] In this embodiment, FKM:PVC=0.6:1.2, other operations are the same as in Example 1, and according to the ASTM-D3359 standard test, the firmness of the composite resin layer and the reinforcing layer is 5B, and the composite resin layer does not fall off from the reinforcing layer. A perfluorosulfonic acid resin film is applied on the composite resin layer, and the perfluorosulfonic acid resin film is not damaged, and its peel strength is 50mN / cm

[0041] Embodiment 3:

[0042] In this embodiment, FKM:PVC=0.6:1.2, DCP dosage is 0.304g, DOP dosage is 0.76g, other operations are the same as in Example 1, and according to ASTM-D3359 standard test, the firmness of the composite resin layer and the reinforcement layer is 5B, and the composite resin layer does not fall off from the reinforcement layer. A perfluorosulfonic acid resin film is applied on the composite resin layer, and the perfluorosulfonic acid resin film is not damaged, and its peel strength is 35mN / cm

[0043] Comparative Example 1:

[0044] In this comparative example, FKM:PVC=4:1, and the amount of DCP is 0.304g, DOP is not added, and the other operation steps are the same as Example 1. According to the ASTM-D3359 standard test, the firmness of the composite resin layer and the reinforcement layer is 3B, and the composite resin layer does not fall off from the reinforcement layer. A perfluorosulfonic acid resin film is applied on the composite resin layer, and the perfluorosulfonic acid resin film is not damaged, and its peel strength is 100mN / cm, which exceeds the standard.

[0045] Comparative Example 2:

[0046] In this comparative example, FKM:PVC=4:1, the amount of DOP is 0.304g, DCP is not added, and the other operation steps are the same as Example 1. According to the ASTM-D3359 standard test, the firmness of the composite resin layer and the reinforcement layer is 3B, and the composite resin layer does not fall off from the reinforcement layer. A perfluorosulfonic acid resin film is coated on the composite resin layer, and the perfluorosulfonic acid resin film is not damaged, and its peel strength is 130mN / cm, which exceeds the standard.

[0047] Comparative Example 3:

[0048] In this comparative example, the composite resin layer in Example 1 is replaced by FKM, the curing temperature is 150° C., the curing time is 80 seconds, and the other operation processes are the same as in Example 1. The FKM layer falls off from the reinforcement layer and cannot be used as a release film.

[0049] Comparative Example 4:

[0050] In this comparative example, the composite resin layer in Example 1 is replaced by PVC, the curing temperature is 100° C., the curing time is 50 seconds, and the other operation processes are the same as in Example 1. The PVC layer falls off from the reinforcement layer and cannot be used as a release film.

[0051] Comparative Example 5:

[0052] In this embodiment, FKM:PVC=0.1:1.2, no DOP and DCP are added, and other operation steps are the same as in Example 1. According to the ASTM-D3359 standard test, the firmness of the composite resin layer and the reinforcement layer is 4B, and the composite resin layer does not fall off from the reinforcement layer. A perfluorosulfonic acid resin film is applied on the composite resin layer, and the perfluorosulfonic acid resin film is not damaged, and its peel strength is 150mN / cm, which exceeds the standard.

[0053] According to the description in the above specification, the technical personnel in the field to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the invention should also fall within the protection scope of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention. Other protective films that are the same or similar to the above are all within the protection scope of the present invention.

Claims

1. A low peel strength fluorine release film, comprising a base layer and a compound resin layer, It is characterized in that The composite resin layer comprises FKM and PVC; The base layer includes a PET substrate layer and a reinforcement layer, the compound resin layer, the reinforcement layer and the PET substrate layer are arranged in order from top to bottom, and the peeling amount between the reinforcement layer and the compound resin layer is 0%; The preparation method of the low peel strength fluorine release film is as follows: (1) Preparation of the reinforcement layer: The PET substrate layer is modified by inputting high-energy particles using a corona treatment system; (2) Dissolution treatment of FKM and PVC: the PVC is dissolved at room temperature, and the FKM is dissolved at 40-60° C. The dissolved FKM solution and PVC solution are mixed, and DCP is added as a solubilizing agent and stirred to obtain a solution A; (3) Curing treatment: coating the solution A obtained in step (2) on the reinforcing layer obtained in step (1), and performing a curing treatment; In step (2), DOP is added as a softener during the dissolution process of the FKM, and the amount used is 5-10 phr; the amount of DCP is 1-4 phr; the amount of FKM is 48-84 phr, and the amount of PVC is 80-100 phr.

2. The low peel strength fluorine release film according to claim 1, It is characterized in that The mass ratio of the FKM to PVC is (0.6-1):1.

2.

3. The low peel strength fluorine release film according to claim 1 or 2, It is characterized in that The composite resin layer can be attached with a perfluorosulfonic acid resin film, and the peel strength of the perfluorosulfonic acid resin film is 20-50 mN / cm.

4. The low peel strength fluorine release film according to claim 1, It is characterized in that The thickness of the PET substrate layer is 50-150 μm, the thickness of the reinforcement layer is 50-100 nm, and the thickness of the compound resin layer is 90-300 nm.

5. The low peel strength fluorine release film according to claim 1, It is characterized in that The energy density of the corona treatment in step (1) is 120-160 W·min / ㎡.

6. The low peel strength fluorine release film according to claim 1, It is characterized in that The solvent of the solution is THF, the concentration of the FKM solution is 0.023 g / ml-0.046 g / ml; the solid content of the solution A is 1-6%, and the viscosity is 2.27-5.81 MPa·S.

7. The low peel strength fluorine release film according to claim 1, It is characterized in that The curing temperature in step (3) is 120° C. and the curing time is 60 s.

Citation Information

Patent Citations

  • Back membrane for perfluorinated proton exchange membrane

    CN209447937U

  • Multifunctional platform

    CN210203836U

  • Fluorine release film and preparation method thereof

    CN112143012A

  • Fluorine release film

    CN210103836U

  • Heat resistant adhesive sheet and manufacturing method of functional film

    JP2016098297A