A comprehensive smelting method for low-grade molybdenum concentrate containing tungsten

By using phosphoric acid as a leaching agent and extraction agent in the oxygen pressure cooking method to separate molybdenum and tungsten, the problems of difficult separation of tungsten and molybdenum and cumbersome processes in traditional smelting processes are solved, and efficient, clean extraction and high purity of low-grade ores are achieved. Preparation of tungsten and molybdenum products.

CN116411183BActive Publication Date: 2024-10-29ZHENGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210648447.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-09
Publication Date
2024-10-29
Estimated Expiration
2042-06-09

AI Technical Summary

Technical Problem

The existing tungsten-containing low-grade molybdenum concentrate smelting process has problems such as difficulty in efficient recovery and separation of tungsten and molybdenum, and cumbersome processes. In particular, the traditional ammonia leaching molybdenum smelting process has high ore grade requirements, and the traditional pressure cooking method leads to the precipitation of molybdenum acid. Coverage affects the smelting effect.

Method used

Phosphoric acid is used as the leaching agent to perform oxygen pressure cooking leaching under the conditions of oxygen pressure and water, and then the extraction agent and ion exchange resin are used to selectively extract and separate molybdenum and tungsten to form an acidic solution for further processing, simplifying the smelting process and improving Recovery rate.

Benefits of technology

It achieves clean extraction of low-grade ores and high-purity preparation of tungsten and molybdenum materials, reduces the consumption of chemical reagents and the complexity of the smelting process, improves the comprehensive recovery rate of molybdenum and tungsten, simplifies the process flow and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116411183B_ABST
    Figure CN116411183B_ABST
Patent Text Reader

Abstract

The present invention relates to a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten, which belongs to the technical field of metal smelting and is used to solve the problems of efficient recovery of low-grade molybdenum concentrate containing tungsten and difficulty in separating tungsten from molybdenum. The method comprises: step 1. under the conditions of oxygen pressure and water, using phosphoric acid as a leaching agent to oxygen-pressure cook and leach the low-grade molybdenum concentrate containing tungsten to achieve the leaching of molybdenum and tungsten; step 2. filtering after leaching to obtain a leachate containing molybdenum and tungsten, and then using an extractant to selectively extract molybdenum from the leachate to obtain a tungsten-containing raffinate and a molybdenum-containing extract to achieve the separation of molybdenum; step 3. using an ion exchange resin or an extractant to extract tungsten from the tungsten-containing raffinate. The method of the present invention can achieve efficient recovery of molybdenum and tungsten from low-grade molybdenum concentrate containing tungsten.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal smelting, and in particular to a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten. Background Art

[0002] my country has large reserves of molybdenum resources, but the resource endowment is poor. Among them, the Yechangping molybdenum mine in Sanmenxia, ​​Lushi, Henan is the most typical. It is a polymetallic deposit dominated by molybdenum and associated with tungsten, fluorite, and magnetite. The surface of this type of deposit is oxidized, and molybdenum exists in the form of a mixture of sulfide and oxidation, containing calcium tungstate, iron tungstate, molybdenum disulfide, calcium molybdate and other tungsten-molybdenum ore phases. Due to the coexistence of oxidized sulfide ores and tungsten and molybdenum ores, this type of deposit is difficult to select and smelt, and its efficient utilization has always been a problem in the industry.

[0003] The existing molybdenum concentrate smelting process mostly adopts the oxidation roasting-ammonia leaching process. A large amount of sulfur dioxide flue gas is generated during the oxidation roasting process, which can not effectively recycle the sulfur element in the molybdenum concentrate and cause a lot of air pollution. At the same time, the temperature control during the roasting process is difficult. If the roasting temperature is too high, the molybdenum will also be lost by sublimation; if the roasting temperature is too low, it will cause incomplete oxidation of the molybdenum, increasing the difficulty of leaching.

[0004] In view of the above reasons, technicians began to seek methods for directly processing molybdenum concentrate, namely atmospheric decomposition and high-pressure decomposition. The atmospheric decomposition method uses strong oxidants such as sodium hypochlorite and potassium permanganate for oxidation leaching. Due to the large amount of strong oxidants used, the reaction process is difficult to control and is prone to explosion hazards, which is not convenient for large-scale application. The high-pressure decomposition method, also known as oxygen pressure cooking, is a very promising process that directly oxidizes and decomposes molybdenum concentrate by introducing oxygen under alkaline or neutral high temperature and high pressure conditions.

[0005] However, in the process of decomposing molybdenum concentrate by the traditional pressure cooking method, most of the molybdenum forms molybdenum acid precipitate. Molybdenum acid is a viscous solid that covers the surface of the molybdenum concentrate ore, which will wrap the unreacted molybdenum concentrate and thus affect the oxidation of molybdenum. The obtained molybdenum acid precipitate also requires a dissolution process with ammonia water or sodium hydroxide. At the same time, a small amount of molybdenum remains in the leaching solution, which requires special molybdenum recovery equipment, making the subsequent recovery process very cumbersome. Summary of the invention

[0006] In view of the above analysis, the present invention aims to provide a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten, which can solve at least one of the following technical problems: (1) The existing low-grade molybdenum concentrate containing tungsten is difficult to efficiently recover and separate tungsten from molybdenum. (2) The existing method for recovering tungsten and molybdenum from low-grade molybdenum concentrate containing tungsten is complicated and has high requirements on the grade of the original ore. For example, the sodium hydroxide pressure cooking method requires a WO3 content of at least 40%; the traditional ammonia leaching molybdenum smelting process requires the ore molybdenum content to be above 50%. The new method proposed in the present invention can realize the clean extraction of low-grade ore and the preparation of tungsten and molybdenum materials.

[0007] The purpose of the present invention is mainly achieved through the following technical solutions:

[0008] The present invention provides a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten, comprising:

[0009] Step 1. Under the conditions of oxygen pressure and water, phosphoric acid is used as a leaching agent to leach low-grade molybdenum concentrate containing tungsten by oxygen pressure cooking to achieve leaching of molybdenum and tungsten;

[0010] Step 2. After leaching, filtering is performed to obtain a leachate containing molybdenum and tungsten, and then molybdenum is selectively extracted from the leachate using an extractant to obtain a tungsten-containing raffinate and a molybdenum-containing extract, thereby separating molybdenum;

[0011] Step 3: extracting tungsten from the tungsten-containing raffinate using ion exchange resin or extractant.

[0012] Furthermore, in step 1, the Mo grade in the low-grade molybdenum concentrate containing tungsten is 3% to 40%, and the grade of WO3 is 3% to 40%.

[0013] Furthermore, in step 1, the low-grade molybdenum concentrate containing tungsten contains a variety of mineral phases, including molybdenum disulfide, molybdenum dioxide, molybdenum trioxide, calcium tungstate, iron tungstate, calcium carbonate and calcium molybdate.

[0014] Furthermore, in step 1, the oxygen pressure is 0.8 MPa to 1.5 MPa.

[0015] Furthermore, in step 1, the oxygen autoclave temperature is 160° C. to 220° C., and the oxygen autoclave time is 2 hours to 5 hours.

[0016] Furthermore, in step 1, the concentration of phosphoric acid is 50 g / L to 180 g / L, and the liquid-to-solid ratio is 5 to 10 L / kg.

[0017] Furthermore, in step 2, the extractant is a cationic extractant, and the cationic extractant contains P204 and / or P507+kerosene, and the volume fraction of P204 and / or P507 is 20% to 50%.

[0018] Furthermore, step 2 also includes using a stripping agent to strip molybdenum from the molybdenum-containing extract to obtain a molybdenum-containing stripping solution.

[0019] Furthermore, in step 3, the tungsten is adsorbed by an anion exchange resin, and then the tungsten is analyzed by an analytical agent.

[0020] Furthermore, in step 3, a neutral extractant is used to extract tungsten from the tungsten-containing raffinate to obtain a tungsten-extracted raffinate and an extractant loaded with tungsten; and a stripping agent is used to strip tungsten from the tungsten-loaded extractant to obtain a stripping solution containing tungsten.

[0021] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0022] (1) The method of the present invention uses phosphoric acid as a leaching agent for oxygen pressure cooking leaching, oxidatively leaching the sulfur element in the tungsten-containing low-grade molybdenum concentrate into sulfuric acid to form an acidic system, and at the same time utilizes the complexation of tungsten and molybdenum with phosphorus in the acidic solution to complete the digestion and leaching of the tungsten-molybdenum mixed ore, and transfer all the valuable tungsten and molybdenum elements into the acidic solution. Compared with the existing tungsten and molybdenum sorting and leaching technology, it effectively utilizes the impurity elements in the mineral, greatly reduces the consumption of chemical reagents, and greatly shortens the smelting process, simplifies the smelting process, and is conducive to improving the comprehensive recovery rate.

[0023] (2) In the present invention, during the leaching process of low-grade molybdenum concentrate containing tungsten using phosphoric acid oxygen autoclave, both iron and calcium enter the slag phase, wherein calcium combines with newly generated sulfuric acid to form calcium sulfate precipitate, and iron is converted into hematite and enters the slag phase. The leaching solution is purified, and the residual solution after tungsten and molybdenum are extracted separately can be directly recycled, thereby greatly saving the reagents used in the process and realizing clean smelting.

[0024] (3) The present invention leaches tungsten and molybdenum together into the solution, and uses the difference in properties of tungsten and molybdenum under acidic conditions to solve the problem of separating large amounts of tungsten and molybdenum by a selective extraction method. Compared with the existing crystallization method or manganese salt precipitation method, the present invention does not require additional separation reagents, the separation and purification process is simpler, and high-purity tungsten and molybdenum products can be directly prepared, further reducing production costs.

[0025] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be achieved and obtained through the contents particularly pointed out in the description. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is a process flow chart of a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten. DETAILED DESCRIPTION

[0027] The preferred embodiments of the present invention are described in detail below. The embodiments are only used to illustrate the principles of the present invention and are not used to limit the scope of the present invention.

[0028] The low-grade molybdenum concentrate containing tungsten in the present invention is a tungsten-molybdenum oxidized sulfide mixed ore. The tungsten-molybdenum oxidized sulfide mixed ore has a complex ore phase. During the decomposition of the molybdenum concentrate by the traditional pressure cooking method, most of the molybdenum forms molybdenum acid precipitates. The molybdenum acid is a viscous solid that covers the surface of the molybdenum concentrate ore, which will wrap the unreacted molybdenum concentrate and further affect the oxidation of molybdenum. The obtained molybdenum acid precipitate also requires a dissolution process of ammonia water or sodium hydroxide. At the same time, a small amount of molybdenum remains in the leaching solution, which requires special molybdenum recovery equipment, making the subsequent recovery process very cumbersome.

[0029] The present invention provides a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten. The process flow chart is as follows: Figure 1 As shown, including:

[0030] Step 1. Under the conditions of oxygen pressure and water, phosphoric acid is used as a leaching agent to oxygen-pressure cook and leach low-grade molybdenum concentrate containing tungsten (referred to as tungsten-molybdenum mixed ore) to achieve leaching of molybdenum and tungsten;

[0031] Step 2. After leaching, the mixture is cooled to room temperature and filtered to obtain a leachate containing molybdenum and tungsten, and then molybdenum is selectively extracted from the leachate using an extractant to obtain a tungsten-containing raffinate and a molybdenum-containing extract, thereby separating molybdenum;

[0032] Step 3: extracting tungsten from the tungsten-containing raffinate using ion exchange resin or extractant.

[0033] Specifically, in step 1, the Mo grade in the low-grade molybdenum concentrate containing tungsten is 3% to 40%, and the grade of WO3 is 3% to 40%.

[0034] Specifically, in the above step 1, the tungsten-containing low-grade molybdenum concentrate contains multiple mineral phases such as molybdenum disulfide, molybdenum dioxide, molybdenum trioxide, calcium tungstate, iron tungstate, calcium carbonate, and calcium molybdate.

[0035] Specifically, in the above step 1, phosphoric acid is used as a leaching agent for oxygen pressure cooking leaching, and the sulfur element in the tungsten-containing low-grade molybdenum concentrate is oxidized and leached to be converted into sulfuric acid to form an acidic system. At the same time, the complexation of tungsten and molybdenum with phosphorus in the acidic solution is utilized to complete the digestion and leaching of the tungsten-molybdenum mixed ore, and all the valuable tungsten and molybdenum elements are transferred to the acidic solution. Compared with the existing tungsten and molybdenum separation and separate leaching technology, the impurity elements in the mineral are effectively utilized, the consumption of chemical reagents is greatly reduced, and the smelting process is greatly shortened, the smelting process is simplified, and it is beneficial to improve the comprehensive recovery rate; in the process of using phosphoric acid oxygen pressure cooking to complete the leaching of the tungsten-containing low-grade molybdenum concentrate, iron and calcium both enter the slag phase, wherein calcium combines with newly generated sulfuric acid to form calcium sulfate precipitation, iron is converted into hematite and enters the slag phase, and the leachate is purified.

[0036] Specifically, in the above step 1, oxygen is the key factor that plays an oxidizing role in the oxygen pressure cooking process. Since the oxygen pressure cooking leaching process is a gas-solid-liquid heterogeneous reaction, the general gas-participated reaction mainly relies on the gas-solid and gas-liquid interface heterogeneous reactions. The gas-participated interface reaction has a slow reaction rate, which seriously affects the efficiency of oxygen pressure cooking leaching. Providing sufficient pressure to oxygen can better dissolve it in the liquid, and generate a gas-solid-liquid heterogeneous reaction at the liquid-solid heterogeneous reaction interface, thereby greatly improving the efficiency of oxygen pressure cooking leaching. Therefore, the oxygen pressure is 0.8Mpa to 1.5Mpa.

[0037] Specifically, in the above step 1, the higher the leaching oxygen pressure cooking temperature, the faster the pressure cooking rate, but it will also cause higher energy consumption. Therefore, considering the production efficiency and energy consumption of pressure cooking comprehensively, the leaching oxygen pressure cooking temperature is determined to be 160°C to 220°C according to the cost-effectiveness ratio.

[0038] Specifically, in the above step 1, the longer the oxygen pressure cooking time is, the more complete the reaction is, but at the same time, too long pressure cooking will cause higher energy consumption. The oxygen pressure cooking time is 2 hours to 5 hours.

[0039] Specifically, in the above step 1, the concentration of phosphoric acid is 50 g / L to 180 g / L, and the liquid-to-solid ratio is 5 to 10 L / kg.

[0040] Specifically, in the above step 2, the extractant is a cationic extractant, and the cationic extractant contains P204 and / or P507+kerosene, wherein the volume fraction of P204 and / or P507 is 20% to 50%.

[0041] Specifically, the above step 2 also includes using a stripping agent to strip molybdenum from the molybdenum-containing extract to obtain a molybdenum-containing stripping solution (i.e., a molybdenum stripping solution).

[0042] Specifically, in the above step 2, it also includes evaporating and crystallizing the molybdenum stripping solution to obtain molybdic acid, and then calcining it to obtain the molybdenum trioxide product.

[0043] Specifically, in the above step 2, the stripping agent is hydrogen peroxide, and the concentration of hydrogen peroxide is 10% to 20%.

[0044] Specifically, in the above step 2, both the extraction and the stripping are countercurrent extraction, and the extraction and stripping stages are both 5 to 15;

[0045] Specifically, in the above step 2, the extraction ratio is an important influencing factor of extraction. When the extraction ratio of molybdenum is less than 1:1, the extraction will be insufficient, and some molybdenum cannot be transferred to the organic phase. Therefore, from the perspective of the recovery rate of molybdenum, the greater the O / A ratio, the more thorough the transfer of molybdenum to the organic phase. However, too much organic phase will also cause the increase of costs such as solvents and processes. After in-depth research, the inventor found that when O / A is greater than 5:1, the extraction cost-effectiveness ratio is seriously reduced. Therefore, the extraction ratio of molybdenum is controlled to be 5:1 to 1:1 compared to O / A, and the stripping ratio is 10:1 to 3:1 compared to O / A.

[0046] Specifically, the above step 3 includes using an anion exchange resin to adsorb tungsten, and then using an analytical agent to analyze the tungsten.

[0047] Specifically, in the above step 3, the anion exchange resins used are primary amine resins, secondary amine resins and tertiary amine resins; and the analytical agents are ammonia water and water.

[0048] Specifically, the above step 3 includes extracting tungsten from the tungsten-containing raffinate using a neutral extractant to obtain a tungsten-extracted raffinate and an extractant loaded with tungsten; stripping tungsten from the tungsten-loaded extractant using a stripping agent to obtain a tungsten-containing stripping solution (i.e., tungsten stripping solution); and returning the tungsten-extracted raffinate to step 1 for recycling.

[0049] Specifically, in the above step 3, the tungsten stripping solution is subjected to a conventional purification process and then evaporated and crystallized to obtain the ammonium paratungstate product.

[0050] Specifically, in the above step 3, the extractant used is a neutral extractant, including one or a mixture of tributyl phosphate, octanol, n-octanol, and decanol, the extractant concentration is 30% to 80%, and the rest is kerosene; the extraction phase ratio O / A for tungsten extraction is 3:1 to 1:2, and the stripping phase ratio O / A is 10:1 to 3:1; both extraction and stripping are countercurrent extraction, and the extraction and stripping stages are 5 to 15; the stripping agent is ammonia water or water, wherein the ammonia concentration is 5 to 8 mol / L. The tungsten extraction residual solution is returned to step 1 and used for oxygen pressure cooking leaching of low-grade molybdenum concentrate containing tungsten.

[0051] Specifically, in the method of the present invention, the leaching rate of molybdenum is above 97%, and the leaching rate of tungsten is above 97%.

[0052] The preferred embodiments of the present invention are described in detail below to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0053] Example 1

[0054] A specific embodiment of the present invention discloses a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten.

[0055] In this embodiment, the main components of the tungsten-containing low-grade molybdenum concentrate are 25.1% (mass percentage) molybdenum and 20.3% (mass percentage) tungsten; the tungsten-containing low-grade molybdenum concentrate contains molybdenum disulfide, molybdenum dioxide, molybdenum trioxide, molybdenum oxide, calcium tungstate, iron tungstate, calcium carbonate, calcium molybdate and other mineral phases.

[0056] The method of this embodiment includes:

[0057] Using phosphoric acid as the leaching agent, the phosphoric acid concentration is 100 g / L, the oxygen partial pressure is 1.2 MPa, the temperature is 160°C, and the liquid-to-solid ratio is 5 L / kg, oxygen pressure leaching is carried out in an autoclave for 5 hours.

[0058] After the oxygen pressure cooking leaching is completed, the leaching solution containing tungsten and molybdenum is obtained by cooling to room temperature and filtering.

[0059] Among them, the leaching rate of molybdenum is 98.5%, and the leaching rate of tungsten is 98.2%.

[0060] For the leachate containing tungsten and molybdenum, firstly, molybdenum is extracted with a cationic extractant P204 with a volume fraction of 40% to obtain P204 loaded with molybdenum. The extraction ratio is O / A=4:1, and the extraction stage is 10 countercurrent stages.

[0061] The molybdenum-loaded P204 is then stripped with 15% hydrogen peroxide to obtain a stripping solution and a raffinate; the stripping ratio is O / A=7:1, and the stripping stage is 7 countercurrent stages.

[0062] The stripping solution is evaporated and crystallized to obtain molybdic acid, which is then calcined to obtain the molybdenum trioxide product.

[0063] The tungsten-containing raffinate after molybdenum extraction uses 80% tributyl phosphate + 20% kerosene as an extractant to extract tungsten, the extraction ratio is O / A = 1:2, and the extraction level is countercurrent 5 levels; 8mol / L ammonia water is used to strip tungsten, the stripping ratio is O / A = 3:1, and the stripping level is countercurrent 5 levels. The tungsten stripping solution is evaporated and crystallized after conventional purification process to obtain ammonium paratungstate product. The recovery rate of tungsten can reach more than 98%. The same effect can be achieved by using 60% tributyl phosphate + 20% octanol + 20% kerosene.

[0064] Example 2

[0065] A specific embodiment of the present invention discloses a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten.

[0066] In this embodiment, the main components of the tungsten-containing low-grade molybdenum concentrate are 40% (mass percentage) molybdenum and 5% (mass percentage) tungsten; the tungsten-containing low-grade molybdenum concentrate contains molybdenum disulfide, molybdenum dioxide, molybdenum trioxide, calcium tungstate, iron tungstate, calcium carbonate, calcium molybdate and other mineral phases.

[0067] The method of this embodiment includes:

[0068] Using phosphoric acid as the leaching agent, the phosphoric acid concentration is 50 g / L, the oxygen partial pressure is 1.5 MPa, the temperature is 200°C, and the liquid-to-solid ratio is 8 L / kg, oxygen pressure leaching is carried out in an autoclave for 3 hours.

[0069] After the oxygen pressure cooking leaching is completed, the leaching solution containing tungsten and molybdenum is obtained by cooling to room temperature and filtering.

[0070] Among them, the leaching rate of molybdenum is 99.5%, and the leaching rate of tungsten is 97.2%.

[0071] For the leachate containing tungsten and molybdenum, firstly, molybdenum is extracted with cationic extractant P507 with a volume fraction of 50% to obtain P507 loaded with molybdenum. The extraction ratio is O / A=5:1, and the extraction stage is 15 countercurrent stages.

[0072] The molybdenum-loaded P507 was stripped with 20% hydrogen peroxide to obtain a stripping solution and a raffinate; the stripping phase ratio was O / A=10:1, and the stripping stage was 5 countercurrent stages.

[0073] The stripping solution is evaporated and crystallized to obtain molybdic acid, which is then calcined to obtain the molybdenum trioxide product.

[0074] The tungsten-containing raffinate after molybdenum extraction is adsorbed by primary amine resin, and tungsten is analyzed by 5 mol / L ammonia water. The recovery rate of tungsten can reach more than 98%. The same effect can be achieved by using secondary amine or tertiary amine resin.

[0075] Example 3

[0076] A specific embodiment of the present invention discloses a comprehensive smelting method for low-grade molybdenum concentrate containing tungsten.

[0077] In this embodiment, the main components of the tungsten-containing low-grade molybdenum concentrate are 5% (mass percentage) molybdenum and 40% (mass percentage) tungsten; the tungsten-containing low-grade molybdenum concentrate contains molybdenum disulfide, molybdenum dioxide, molybdenum trioxide, calcium tungstate, iron tungstate, calcium carbonate, calcium molybdate and other mineral phases.

[0078] The method of this embodiment includes:

[0079] Using phosphoric acid as the leaching agent, the phosphoric acid concentration is 180g / L, the oxygen partial pressure is 0.8Mpa, the temperature is 220°C, and the liquid-to-solid ratio is 10L / kg, oxygen pressure leaching is carried out in an autoclave for 2 hours.

[0080] After the oxygen pressure cooking leaching is completed, the leaching solution containing tungsten and molybdenum is obtained by cooling to room temperature and filtering.

[0081] Among them, the leaching rate of molybdenum is 97.5%, and the leaching rate of tungsten is 99.2%.

[0082] For the leaching solution containing tungsten and molybdenum, 10% P204+10% P507+80% kerosene is first used as an extractant to extract molybdenum to obtain an organic phase loaded with molybdenum. The extraction phase ratio is O / A=1:1, and the extraction stage is 5 countercurrent stages.

[0083] The molybdenum-loaded extractant is then stripped with 10% hydrogen peroxide to obtain a stripping solution and a raffinate; the stripping phase ratio is O / A=3:1, and the stripping stage is 5 countercurrent stages.

[0084] The stripping solution is evaporated and crystallized to obtain molybdic acid, which is then calcined to obtain the molybdenum trioxide product.

[0085] The tungsten-containing raffinate after molybdenum extraction is extracted with 30% 2-octanol + 70% kerosene as the extractant, the extraction phase ratio is O / A=1:2, and the extraction stage is 15 stages of countercurrent; pure water is used to strip tungsten, the stripping phase ratio is O / A=7:1, and the stripping stage is 15 stages of countercurrent. The recovery rate of tungsten can reach more than 98%, and the same effect can be achieved by using octanol or decanol.

[0086] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A comprehensive smelting method for low-grade molybdenum concentrate containing tungsten, characterized in that: include: Step 1. Under the conditions of oxygen pressure and water, phosphoric acid is used as a leaching agent to leach low-grade molybdenum concentrate containing tungsten by oxygen pressure cooking to achieve leaching of molybdenum and tungsten; Step 2. After leaching, filtering is performed to obtain a leachate containing molybdenum and tungsten, and then molybdenum is selectively extracted from the leachate using an extractant to obtain a tungsten-containing raffinate and a molybdenum-containing extract, thereby separating molybdenum; Step 3. extracting tungsten from the tungsten-containing raffinate using an ion exchange resin or an extractant; In the step 1, the low-grade molybdenum concentrate containing tungsten contains a variety of mineral phases, including molybdenum disulfide, molybdenum dioxide, molybdenum trioxide, calcium tungstate, iron tungstate, calcium carbonate and calcium molybdate; In step 1, the oxygen pressure is 0.8 MPa to 1.5 MPa; the oxygen autoclave temperature is 160° C. to 220° C.; the oxygen autoclave time is 2 hours to 5 hours; the phosphoric acid concentration is 50 g / L to 180 g / L, and the liquid-to-solid ratio is 5 to 10 L / kg.

2. The method according to claim 1, characterized in that In the step 1, the Mo grade in the low-grade molybdenum concentrate containing tungsten is 3% to 40%, and the grade of WO3 is 3% to 40%.

3. The method according to claim 1, characterized in that In step 1, the oxygen pressure is 0.8Mpa~1.2Mpa.

4. The method according to claim 1, characterized in that: In the step 1, the oxygen autoclave temperature is 160° C. to 200° C., and the oxygen autoclave time is 3 hours to 5 hours.

5. The method according to claim 1, characterized in that In step 1, the concentration of phosphoric acid is 100 g / L to 180 g / L, and the liquid-to-solid ratio is 5 to 8 L / kg.

6. The method according to claim 1, characterized in that In step 2, the extractant is a cationic extractant, and the cationic extractant contains P204 and / or P507+kerosene, wherein the volume fraction of P204 and / or P507 is 20% to 50%.

7. The method according to claim 1, characterized in that The step 2 also includes using a stripping agent to strip molybdenum from the molybdenum-containing extract to obtain a molybdenum-containing stripping solution.

8. The method according to any one of claims 1 to 7, characterized in that: The step 3 includes using an anion exchange resin to adsorb tungsten, and then using an analytical agent to analyze the tungsten.

9. The method according to any one of claims 1 to 7, characterized in that: The step 3 comprises extracting tungsten from the tungsten-containing raffinate using a neutral extractant to obtain a tungsten-extracted raffinate and an extractant loaded with tungsten; and stripping tungsten from the tungsten-loaded extractant using a stripping agent to obtain a stripping solution containing tungsten.

Citation Information

Patent Citations

  • Process for separating molybdenum and nickel form black shale containing molybdenum and nickel

    CN101289702A

  • Molybdenum cleaning metallurgy method

    CN108396141A