A novel electro-variable infrared emissivity device and its preparation method

By using doped zinc oxide nanocrystals and electrochemical methods to control localized surface plasmon resonance in infrared stealth technology, the problem of insufficient control capabilities in the infrared band in the existing technology has been solved, and efficient control of the 3-14 μm infrared band has been achieved. and the transparency of the device, which enhances the application potential of infrared stealth technology.

CN116430631BActive Publication Date: 2024-10-29NAT UNIV OF DEFENSE TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310131473.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-17
Publication Date
2024-10-29
Estimated Expiration
2043-02-17

Smart Images

  • Figure CN116430631B_ABST
    Figure CN116430631B_ABST
Patent Text Reader

Abstract

The invention discloses a novel electro-variable infrared emissivity device and a preparation method thereof. The electro-variable infrared emissivity device comprises, from top to bottom, an infrared transparent substrate layer, a variable infrared emissivity functional layer, an infrared high reflection layer, an electrolyte layer, an ion storage layer and a counter electrode layer; the infrared high reflection layer and the counter electrode layer are connected to a positive electrode and a negative electrode respectively; the variable infrared emissivity functional layer is doped zinc oxide nanocrystals, the doped ions in the doped zinc oxide nanocrystals are trivalent metal ions, and the doping amount of the trivalent metal ions is 0.1-10%. The novel electro-variable infrared emissivity device prepared by the invention utilizes localized surface plasmon resonance to realize the regulation of the infrared band of 2.5-14 μm by an electrochemical method, and has the characteristics of a large regulation range, rapid response and long cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of infrared stealth technology, and in particular relates to a novel electrovariable infrared emissivity device and a preparation method thereof. Background Art

[0002] The infrared radiation characteristics of a target are mainly affected by temperature and emissivity. The higher the temperature or emissivity of a target, the stronger its infrared radiation characteristics. Therefore, adjusting the target emissivity to adjust the infrared characteristics has become an important means of infrared stealth technology. Electrovariable emissivity devices have the advantages of a wide range of emissivity adjustment, fast response speed, and flexible response, and have great application potential in the field of infrared stealth technology.

[0003] Localized Surface Plasmon Resonance (LSPR) refers to the phenomenon that when light is incident on nanoparticles with good conductivity, if the incident photon frequency matches the oscillation frequency of the nanoparticles, the nanoparticles will have a strong absorption effect on the photon energy, and localized surface plasmon resonance will occur. At this time, a strong resonance absorption peak will appear in the spectrum. The research on LSPR was initially focused on metal nanoparticles, and LSPR is mainly located in the visible light band. In recent years, the research on semiconductor oxide nanocrystals is in the ascendant, and LSPR is mainly located in the near-infrared (800-3000nm) band, but there is currently no research on electrochemical regulation of LSPR in the infrared band of 3 to 14μm. Summary of the invention

[0004] In order to overcome the technical problems in the prior art, the present invention provides a novel electrovariable infrared emissivity device and a preparation method thereof, which utilizes localized surface plasmon resonance to achieve electrochemical regulation of the 2.5-14 μm infrared band, and has the characteristics of a wide adjustment range, rapid response and long cycle life.

[0005] In order to solve the above technical problems, the technical solutions proposed by the present invention are as follows:

[0006] The first aspect of the present invention provides a novel electro-variable infrared emissivity device, which comprises, from top to bottom, an infrared transparent substrate layer, a variable infrared emissivity functional layer, an infrared high reflective layer, an electrolyte layer, an ion storage layer and a counter electrode layer, wherein the infrared high reflective layer and the counter electrode layer are connected to a positive electrode and a negative electrode, respectively, and the variable infrared emissivity functional layer is doped zinc oxide nanocrystals, wherein the doped ions in the doped zinc oxide nanocrystals are trivalent metal ions, and the doping amount of the trivalent metal ions is 0.1 to 10%.

[0007] The novel electro-variable infrared emissivity device prepared in the present invention uses doped zinc oxide nanocrystals as a variable infrared emissivity functional layer, and controls the doping amount of trivalent metal ions to be 0.1-10%, so that the localized surface plasmon resonance (LSPR) absorption peak of the doped zinc oxide nanocrystals is located in the infrared band of 3-14 μm. Electrochemical injection and extraction of electrons are used to enhance and weaken the LSPR absorption peak, thereby realizing the regulation of infrared emissivity by doped zinc oxide nanocrystals. When negative electricity is applied, electrons are injected into the doped zinc oxide nanocrystal layer, the LSPR absorption peak is enhanced, and the device exhibits high infrared emissivity characteristics. When positive electricity is applied, electrons are extracted from the doped zinc oxide nanocrystal layer, the LSPR absorption peak is weakened, the doped zinc oxide nanocrystal layer exhibits high transmittance, and the device exhibits the high reflection characteristics of the infrared high reflection layer, that is, the low emissivity state, thereby realizing the regulation of infrared emissivity.

[0008] As an optional implementation, in the electrovariable infrared emissivity device provided by the present invention, the thickness of the variable infrared emissivity functional layer is 0.1 to 20 μm.

[0009] As an optional implementation, in the electrotropic infrared emissivity device provided by the present invention, the diameter of the aluminum-doped zinc oxide nanocrystals is 2 to 30 nm.

[0010] As an optional implementation, in the electrotropic infrared emissivity device provided by the present invention, the diameter of the aluminum-doped zinc oxide nanocrystals is 2 to 16 nm.

[0011] As an optional implementation, in the electrovariable infrared emissivity device provided by the present invention, the LSPR absorption peak of the aluminum-doped zinc oxide nanocrystal is located at 3 to 14 μm.

[0012] As an optional implementation, in the electrovariable infrared emissivity device provided by the present invention, the trivalent metal ion is one of aluminum ion, boron ion, gallium ion or indium ion.

[0013] The n-type semiconductor nanocrystal based on ZnO in the present invention generally has a dopant comprising boron ions (B 3+ ), aluminum ions (Al 3+ ), gallium ions (Ga 3+ ) and indium ions (In 3+ ), LSPR absorption will occur in the 3-14μm band, and the LSPR absorption peak of ZnO-based n-type semiconductor nanocrystals can be further regulated by electrochemical means, thereby achieving regulation of infrared emissivity.

[0014] As an optional embodiment, in the electrovariable infrared emissivity device provided by the present invention, the infrared transparent substrate layer material is selected from one of BaF2, CaF2, polypropylene, polyethylene, polytetrafluoroethylene, nylon or silicon wafer.

[0015] The infrared transparent substrate layer in the present invention provides support for the infrared emissivity layer doped with zinc oxide nanocrystals, and at the same time, when a transparent material is selected, the penetration of visible light and infrared light is ensured.

[0016] As an optional implementation, in the electrovariable infrared emissivity device provided by the present invention, the infrared high reflective layer is selected from one of a metal film, an ITO film, an AZO film, a FTO film, and a Mxene film.

[0017] The infrared high reflective layer in the present invention serves as the working electrode of the device and also as the infrared high reflectivity backing. If a transparent material is selected, the transmission of visible light and the high reflection of infrared light can be ensured.

[0018] As an optional implementation, in the electrovariable infrared emissivity device provided by the present invention, the ion storage layer is one of a Pt nanocrystalline layer, an AZO film, a NiO film, and a V2O5 film.

[0019] In the present invention, an ion storage layer is provided, and the material can be selected from platinum nanocrystals, cerium dioxide nanocrystals or aluminum-doped zinc oxide nanocrystals, and its function is to balance the charge change in the process of regulating the infrared emissivity.

[0020] As an optional embodiment, in the electrovariable infrared emissivity device provided by the present invention, the counter electrode layer is selected from one of ITO glass, AZO glass, ITO flexible film, AZO flexible film, carbon nanotube film, metal mesh glass or metal mesh film.

[0021] The transparent counter electrode layer in the present invention serves as the counter electrode and the base support layer of the electrotropic infrared emissivity device. If a transparent material is selected, the transmittance of visible light can be ensured at the same time.

[0022] As an optional implementation, in the electrovariable infrared emissivity device provided by the present invention, the electrolyte layer does not need to be specifically limited, and any electrolyte can be used. In specific use, lithium-based electrolytes and sodium-based electrolytes can be selected.

[0023] In the electrovariable infrared emissivity device of the present invention, when transparent materials are selected for the infrared transparent substrate layer, the infrared high reflective layer and the transparent counter electrode layer, and doped zinc oxide nanocrystals are used as the variable infrared emissivity functional layer, each film layer in the prepared device is a visible light transparent material, so that the prepared electrovariable infrared emissivity device has a certain optical transparency.

[0024] As an optional implementation, in the electrotropic infrared emissivity device provided by the present invention, the control amount of the electrotropic infrared emissivity device for the infrared band of 3 to 5 μm is 0.1 to 6.

[0025] As an optional implementation, in the electrotropic infrared emissivity device provided by the present invention, the control amount of the infrared emissivity of the electrotropic infrared emissivity device for 8 to 14 μm is 0.1 to 6.

[0026] As an optional implementation, in the electrotropic infrared emissivity device provided by the present invention, the control amount of the electrotropic infrared emissivity device in the infrared band of 5 to 8 μm is 0.46.

[0027] As an optional implementation, in the electrotropic infrared emissivity device provided by the present invention, the transmittance of the electrotropic infrared emissivity device to visible light is less than 85%.

[0028] A second aspect of the present invention provides a method for preparing the novel electrovariable infrared emissivity device, comprising the following steps:

[0029] S1. Preparation of upper layer semi-device:

[0030] An infrared transparent base layer material is selected, and a doped zinc oxide nanocrystal dispersion liquid with a trivalent metal ion doping amount of 0.1 to 10% is spin-coated onto the infrared transparent base layer material until the doped zinc oxide nanocrystal thickness is 0.1 to 10 μm. A thin film material is then evaporated on the upper surface of the doped zinc oxide nanocrystal as an infrared high reflection layer, and electrode leads are led out from the infrared high reflection layer thin film to prepare an upper semiconductor device.

[0031] S2. Preparation of lower layer semi-device:

[0032] The material for the counter electrode layer is selected, the dispersion for ion storage is spin-coated onto the material for the counter electrode layer, and the electrode lead is led out from the counter electrode layer to prepare the lower layer semi-device.

[0033] S3. Preparation of new electro-variable infrared emissivity device:

[0034] The upper half device prepared in S1 and the lower half device prepared in S2 are bonded together by transparent silicone rubber, and the electrolyte solution is injected into the middle to obtain a novel electrovariable infrared emissivity device.

[0035] As an optional embodiment, in the preparation method provided by the present invention, the preparation process of the doped zinc oxide nanocrystal dispersion in step S1 is: zinc acetate and the metal organic complex are dissolved in oleic acid, degassed at 70 to 150° C. for 20 to 60 minutes, and then oleylamine is added, and a metal precursor is obtained after further degassing, and then an excess of oleyl alcohol solution is stirred and heated to 260 to 320° C., and the metal precursor is added to the oleyl alcohol solution under a nitrogen atmosphere. After reacting for 1 to 3 hours, nanocrystals are obtained, and the nanocrystals are washed with a toluene / ethanol solution, and then the nanocrystals are dispersed in a toluene solvent to obtain a doped zinc oxide nanocrystal dispersion.

[0036] As an optional embodiment, in the preparation method provided by the present invention, as an optional embodiment, in the preparation method provided by the present invention, the metal organic complex is selected from one of aluminum acetylacetonate, triethylaluminum, aluminum acetate, acetylacetonate boron, triethylboron, boron acetate, gallium acetylacetonate, triethylgallium, gallium acetate, indium acetylacetonate, triethylindium, and indium acetate.

[0037] As an optional embodiment, in the preparation method provided by the present invention, after the doped zinc oxide nanocrystals are spin-coated onto the infrared transparent substrate layer material in step S1, the infrared transparent substrate / doped zinc oxide nanocrystals are heated in an argon environment at 250° C. for 30 minutes.

[0038] As an optional embodiment, in the preparation method provided by the present invention, the electrolyte solution in step S3 is a 1M solution of lithium bis(trifluoromethanesulfonyl)imide in tetraethylene glycol dimethyl ether.

[0039] As an optional embodiment, in the preparation method provided by the present invention, the spin coating process in step S1 is: spin coating at 200-1000 rpm for 10s-60s, then spin coating at 2000-4000 rpm for 5s-20s, and the above process is repeated 5-20 times.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) The electro-variable infrared emissivity device of the present invention uses doped zinc oxide nanocrystals as the variable infrared emissivity material, and at the same time, by controlling the doping amount of trivalent metal ions to 0.1-10%, the localized surface plasmon resonance (LSPR) absorption peak of the doped zinc oxide nanocrystals is located in the 3-14 μm infrared band. By using the electrochemical injection and extraction of electrons to enhance and weaken the LSPR absorption peak, the regulation of the 3-14 μm infrared band is achieved.

[0042] (2) In the electrovariable infrared emissivity device prepared in the present invention, by using doped zinc oxide nanocrystals as the variable infrared emissivity functional layer, when the materials of the infrared transparent substrate layer, the infrared high reflective layer and the counter electrode layer have a certain visible light transmittance, each film layer in the prepared device is a visible light transparent material, and a transparent electrovariable infrared emissivity device can be prepared. The present invention prepares a transparent electrovariable infrared emissivity device for the first time.

[0043] (3) The control amount of the electrotropic infrared emissivity film in the infrared band of 3 to 5 μm is 0.1 to 0.6, and the control amount of the infrared emissivity of 8 to 14 μm is 0.1 to 0.6, the fast response time is less than 600 ms, and the cyclicity is greater than 10,000 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0045] Figure 1 It is a schematic diagram of the structure of the electrovariable infrared emissivity device in the present invention;

[0046] Figure 2 is the LSPR absorption peak of the aluminum-doped zinc oxide nanocrystals prepared in Example 1;

[0047] Figure 3 The morphology and diameter distribution results of the aluminum-doped zinc oxide nanocrystals prepared in Example 1;

[0048] Figure 4 The cross-sectional morphology test result of the upper half device prepared in Example 1;

[0049] Figure 5 The visible light and infrared spectrum test results of the electrovariable infrared emissivity device prepared in Example 1;

[0050] Figure 6 The infrared spectrum test result of the electrovariable infrared emissivity device prepared in Example 2;

[0051] Figure 7 The response time test result of the electrovariable infrared emissivity device prepared in Example 1;

[0052] Figure 8 The following are the cycle performance test results of the electrovariable infrared emissivity device prepared in Example 1.

[0053] Reference numerals:

[0054] 1. Infrared transparent base layer; 2. Variable infrared emissivity functional layer; 3. Infrared high reflection layer; 4. Electrolyte layer; 5. Ion storage layer; 6. Counter electrode layer. DETAILED DESCRIPTION

[0055] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0056] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0057] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0058] The present invention provides a novel electro-variable infrared emissivity device, the structural schematic diagram of which is shown in FIG. Figure 1 As shown, the electrovariable infrared emissivity device is a multilayer structure, which includes, from top to bottom, an infrared transparent substrate layer 1, a variable infrared emissivity functional layer 2, an infrared high reflective layer 3, an electrolyte layer 4, an ion storage layer 5 and a counter electrode layer 6, wherein the infrared high reflective layer 3 and the counter electrode layer 6 are connected to the positive and negative electrodes, respectively; the variable infrared emissivity functional layer 2 is doped zinc oxide nanocrystals, wherein the doped ions are trivalent metal ions, and the doping amount of the trivalent metal ions in the doped zinc oxide nanocrystals is 0.1-10%.

[0059] The thickness of the variable infrared emissivity functional layer in the present invention is 0.1-10 μm.

[0060] Specifically, the diameter of the aluminum-doped zinc oxide nanocrystal is 2-30 nm, preferably 2-16 nm, and the LSPR absorption peak of the aluminum-doped zinc oxide nanocrystal is located at 3-14 μm.

[0061] like Figure 1As shown, the device can switch between a high emissivity state in which electrons are injected into doped zinc oxide nanocrystals and a low emissivity state in which electrons are extracted from doped zinc oxide nanocrystals. The infrared emissivity of the doped zinc oxide nanocrystal film is regulated by electrochemically injecting and extracting electrons to enhance and weaken the LSPR absorption peak. When negative electricity is applied, electrons are injected into the doped zinc oxide nanocrystal layer, the LSPR absorption peak is enhanced, and the device exhibits high infrared emissivity characteristics. When positive electricity is applied, electrons are extracted from the doped zinc oxide nanocrystal layer, the LSPR absorption peak is weakened, the doped zinc oxide nanocrystal layer exhibits high transmittance, and the device exhibits the high reflection characteristics of the infrared high reflection layer, that is, the low emissivity state, thereby achieving the regulation of infrared emissivity.

[0062] In the present invention, the preparation process of doped zinc oxide nanocrystals is as follows:

[0063] First, a metal precursor is prepared, specifically, zinc acetate (15.9-14.4 mmol) and a metal organic complex (0.1-1.6 mmol) are dissolved in 32 mL of oleic acid, degassed at 110° C. for 1 hour, and then 16 ml of oleylamine is added, and further degassed at 70-150° C. for 20-60 min to obtain a metal precursor; then 160 ml of oleyl alcohol is added to a three-necked round-bottom flask, and heated to 260-320° C. under strong stirring, and 45 ml (15 mmol) of the metal precursor is added using a syringe pump under a nitrogen atmosphere at an injection speed of 3 ml / min. After reacting for 1 hour, nanocrystals are obtained, and after the nanocrystals are washed with a toluene / ethanol solution, the nanocrystals are dispersed in a toluene solvent to obtain an aluminum-doped zinc oxide nanocrystal dispersion.

[0064] The infrared transparent substrate layer 1 has a thickness of 0.1 to 1 mm, and the material is selected from one of BaF2, CaF2, polypropylene, polyethylene, polytetrafluoroethylene, nylon or silicon wafer. The infrared transparent substrate layer is used to provide support for the doped zinc oxide nanocrystal variable infrared emissivity layer, and its infrared transmittance is greater than 80%, which can ensure the penetration of infrared light.

[0065] The infrared high reflective layer 3 material is selected from metal film, ITO film, AZO film, FTO film, and Mxene film. As the working electrode of the device and as the infrared high reflectivity backing, its infrared emissivity is greater than 80%, which can ensure the penetration of infrared light.

[0066] The electrolyte layer 4 does not need to be specifically limited, as long as it is an electrolyte, it can be realized. In the specific use process, a lithium-based electrolyte or a sodium-based electrolyte can be selected.

[0067] The ion storage layer 5 is selected from one of a Pt nanocrystalline layer, an AZO film, a NiO film, and a V2O5 film, and its function is to balance the charge change during the infrared emissivity regulation process.

[0068] The material of the counter electrode layer 6 is selected from ITO glass, AZO glass, ITO flexible film, AZO flexible film, carbon nanotube film, metal grid glass or metal substrate, and serves as the counter electrode and substrate support layer of the electrotropic infrared emissivity device.

[0069] The electrovariable infrared emissivity device of the present invention has a regulation value of 0.1-0.6 for the infrared band of 3-5 μm, a regulation value of 0.1-0.6 for the infrared band of 8-14 μm, a regulation value of 0.46 for the infrared band of 5-8 μm, and a transmittance to visible light of less than 85%.

[0070] When the visible light transmittance of the infrared transparent substrate layer 1 and the infrared high reflective layer 3 at 400-760nm is greater than 80%, the infrared transmittance at 2.5-14μm is greater than 80%, and the visible light transmittance of the electrode layer 6 at 400-760nm is greater than 80%, the visible light transmittance of the electrotropic infrared emissivity device can be guaranteed.

[0071] Example 1

[0072] (1) Preparation of aluminum-doped zinc oxide nanocrystalline dispersion:

[0073] Zinc acetate (15.84mmol) and aluminum acetylacetonate (0.16mmol) were dissolved in 32mL oleic acid (the doping amount of aluminum was 1%). Degassing was carried out at 110°C for 1 hour, and then 16mL oleylamine was added, and further degassing was carried out at this temperature for 15 minutes to obtain a metal precursor. Excess oleyl alcohol (160mL) was heated to 280°C under strong stirring in a 250mL three-necked round-bottom flask, and 45mL (15mmol) of the metal precursor was slowly added using a syringe pump at an injection speed of 3mL / min. Nitrogen was filled at the same time, and the nitrogen flow rate was 20L / hour to facilitate the removal of excess water vapor formed. Nanocrystals were obtained after 1h of reaction. After the nanocrystals were washed with a toluene / ethanol solution, the nanocrystals were dispersed in a toluene solvent to obtain an aluminum-doped zinc oxide nanocrystal dispersion.

[0074] (2) Preparation of upper semiconductor devices:

[0075] A BaF2 transparent substrate material with a thickness of 1 mm was selected, and the aluminum-doped zinc oxide nanocrystal dispersion prepared in (1) was spin-coated on the BaF2 substrate at a spin-coating speed of 1000 rpm for 60 s, followed by 4000 rpm for 20 s and the above spin-coating process was repeated until the film thickness reached 1.1 μm. The BaF2 / AZO nanocrystals were heated in an argon environment at 250°C for 30 minutes. An ITO film of about 330 nm was evaporated onto the sample at a deposition rate of 1 A / s using an electron beam evaporation coating machine as an infrared high reflective layer, i.e., a working electrode. The substrate temperature was set to 300°C and the oxygen flow rate was 20 sccm. A 0.1 mm silver wire was attached to one side of the semi-device using a transparent double-sided tape and compacted to ensure full contact between the silver wire and the ITO film to ensure good conductivity.

[0076] (3) Preparation of lower layer semi-device:

[0077] ITO glass was selected as the counter electrode material, and 700nm AZO nanocrystal dispersion was spin-coated on the counter electrode ITO glass as an ion storage layer. One side of the ion storage layer was wiped off to expose the ITO glass substrate. A 0.1mm silver wire was tightly attached to the ITO glass substrate with a transparent double-sided tape, so that the silver wire was in full contact with the ITO glass substrate to ensure good conductivity.

[0078] (4) Preparation of new electro-variable infrared emissivity devices:

[0079] The upper half device and the lower half device are bonded together by transparent silicone rubber, and 0.3 ml of 1 mol lithium bis(trifluoromethanesulfonyl)imide tetraethylene glycol dimethyl ether solution is injected into the middle by using a syringe to obtain a novel electrovariable infrared emissivity device.

[0080] In the novel electrovariable infrared emissivity device prepared in this embodiment, the infrared transparent substrate layer is BaF2, and its visible light transmittance of 400-760nm is 97%, and its infrared transmittance of 2.5-14μm is 96%.

[0081] The variable infrared emissivity functional layer is AZO nanocrystals, and detection is performed using an inductively coupled plasma optical emission spectrometer (ICP-OES, Agilent 720ES), and the aluminum doping content of the AZO nanocrystals is 0.97%.

[0082] The infrared high reflection layer is an AZO film, whose visible light transmittance of 400-760nm is 95%, and the infrared reflectivity of 2.5-14μm is 86%.

[0083] The electrolyte layer was a 1 mol solution of lithium bis(trifluoromethanesulfonyl)imide in tetraethylene glycol dimethyl ether.

[0084] The ion storage layer is AZO film.

[0085] The counter electrode layer is ITO glass, and its visible light transmittance of 400-760nm is 91.4%, and its resistance value is 15Ω / sq.

[0086] The prepared novel electrovariable infrared emissivity device is a transparent device, and its visible light transmittance is 84.7%.

[0087] Example 2

[0088] (1) Preparation of aluminum-doped zinc oxide nanocrystalline dispersion:

[0089] Dissolve zinc acetate (14.4mmol) and aluminum acetylacetonate (1.6mmol) in 32mL oleic acid (aluminum doping amount is 10%). Degas at 110°C for 1 hour, then add 16ml oleylamine, and further degas at this temperature for 15 minutes to obtain a metal precursor. Excess oleyl alcohol (160mL) is heated to 280°C in a 250mL three-necked round-bottom flask under strong stirring, and 45ml (15mmol) of the metal precursor is slowly added using a syringe pump at an injection speed of 3ml / min. At the same time, nitrogen is filled in at a nitrogen flow rate of 20 liters / hour to facilitate the removal of excess water vapor formed. Nanocrystals are obtained after 1h of reaction. After washing the nanocrystals with toluene / ethanol solution, the nanocrystals are dispersed in toluene solvent to obtain aluminum-doped zinc oxide nanocrystal dispersion.

[0090] (2) Preparation of upper semiconductor devices:

[0091] A CaF2 transparent substrate material with a thickness of 1 mm was selected, and the aluminum-doped zinc oxide nanocrystal dispersion prepared in (1) was spin-coated on the CaF2 substrate at a spin-coating speed of 800 rpm for 60 s, followed by 3000 rpm for 20 s, and the above spin-coating process was repeated until the film thickness reached 5 μm. The CaF2 / AZO nanocrystals were heated in an argon environment at 250°C for 30 minutes. An AZO film of about 330 nm was evaporated onto the sample at a deposition rate of 1 A / s using an electron beam evaporation coating machine as an infrared high reflective layer, i.e., a working electrode. The substrate temperature was set to 300°C and the oxygen flow rate was 20 sccm. A 0.1 mm silver wire was attached to one side of the semi-device using a transparent double-sided tape and compacted to ensure full contact between the silver wire and the AZO film to ensure good conductivity.

[0092] (3) Preparation of lower layer semi-device:

[0093] AZO glass was selected as the counter electrode material, and a 700nm AZO nanocrystal dispersion was spin-coated on the counter electrode AZO glass as an ion storage layer. One side of the ion storage layer was wiped off to expose the AZO glass substrate. A 0.1mm silver wire was tightly attached to the AZO glass substrate with a transparent double-sided tape, so that the silver wire was in full contact with the AZO glass substrate to ensure good conductivity.

[0094] (4) Preparation of new electro-variable infrared emissivity devices:

[0095] The upper half device and the lower half device are bonded together by transparent silicone rubber, and 0.3 ml of 1 mol lithium bis(trifluoromethanesulfonyl)imide tetraethylene glycol dimethyl ether solution is injected into the middle by using a syringe to obtain a novel electrovariable infrared emissivity device.

[0096] In the novel electrovariable infrared emissivity device prepared in this embodiment, the infrared transparent substrate layer is CaF2, and its visible light transmittance of 400-760nm is 97%, and its infrared transmittance of 2.5-14μm is 92%.

[0097] The variable infrared emissivity functional layer is AZO nanocrystals, and detection by inductively coupled plasma optical emission spectrometer (ICP-OES, Agilent 720ES) shows that the aluminum doping content of the AZO nanocrystals is 5.79%.

[0098] The infrared high reflection layer is an AZO film, whose visible light transmittance of 400-760nm is 87%, and the infrared reflectivity of 2.5-14μm is 86%.

[0099] The electrolyte layer was a 1 mol solution of lithium bis(trifluoromethanesulfonyl)imide in tetraethylene glycol dimethyl ether.

[0100] The ion storage layer is AZO film.

[0101] The counter electrode layer is AZO glass, and its visible light transmittance in the range of 400-760 nm is 87%, and its resistance is 15Ω / sq.

[0102] The prepared novel electrovariable infrared emissivity device is a transparent device with a visible light transmittance of 78%.

[0103] Example 3

[0104] (1) Preparation of aluminum-doped zinc oxide nanocrystalline dispersion:

[0105] Dissolve zinc acetate (15.2mmol) and aluminum acetylacetonate (0.8mmol) in 32mL oleic acid (aluminum doping level is 5%). Degas at 110°C for 1 hour, then add 16mL oleylamine, and further degas at this temperature for 15 minutes to obtain a metal precursor. Excess oleyl alcohol (160mL) is heated to 280°C in a 250mL three-necked round-bottom flask under strong stirring, and 45mL (15mmol) of the metal precursor is slowly added using a syringe pump at an injection rate of 3mL / min. At the same time, nitrogen is charged at a nitrogen flow rate of 20L / hour to facilitate the removal of excess water vapor formed, and nanocrystals are obtained after 1h of reaction. After washing the nanocrystals with toluene / ethanol solution, the nanocrystals are dispersed in toluene solvent to obtain aluminum-doped zinc oxide nanocrystal dispersion.

[0106] (2) Preparation of upper semiconductor devices:

[0107] A polypropylene film transparent substrate material with a thickness of 1 mm was selected, and the aluminum-doped zinc oxide nanocrystal dispersion prepared in (1) was spin-coated on the polypropylene film substrate at a spin-coating speed of 400 rpm for 60 s, followed by 2000 rpm for 20 s, and the above spin-coating process was repeated until the film thickness reached 5 μm. The polypropylene / AZO nanocrystals were heated in an argon environment at 250°C for 30 minutes. An ITO film of about 330 nm was evaporated onto the sample at a deposition rate of 1 A / s using an electron beam evaporation coating machine as an infrared high reflective layer, i.e., a working electrode. The substrate temperature was set to 300°C and the oxygen flow rate was 20 sccm. A 0.1 mm silver wire was attached to one side of the semi-device using a transparent double-sided tape and compacted to ensure that the silver wire was in full contact with the ITO film to ensure good conductivity.

[0108] (3) Preparation of lower layer semi-device:

[0109] The carbon nanotube film was selected as the counter electrode material, and a 700nm platinum nanocrystal dispersion was spin-coated on the counter electrode carbon nanotube film as an ion storage layer. One side of the ion storage layer was wiped off to expose the carbon nanotube film substrate. A 0.1mm silver wire was tightly attached to the carbon nanotube film substrate with a transparent double-sided tape, so that the silver wire was in full contact with the carbon nanotube film substrate to ensure good conductivity.

[0110] (4) Preparation of new electro-variable infrared emissivity devices:

[0111] The upper half device and the lower half device are bonded together by transparent silicone rubber, and 0.3 ml of 1 mol tetraethylene glycol dimethyl ether solution of lithium bis(trifluoromethanesulfonyl)imide is injected into the middle by using a syringe to obtain a novel electrovariable infrared emissivity device.

[0112] In the novel electrovariable infrared emissivity device prepared in this embodiment, the infrared transparent substrate layer is polypropylene, and its visible light transmittance at 400-760 nm is 93%, and its infrared transmittance at 2.5-14 μm is 84%.

[0113] The variable infrared emissivity functional layer is AZO nanocrystals, and the aluminum doping amount of the AZO nanocrystals is 3.5% as detected by inductively coupled plasma optical emission spectrometer (ICP-OES, Agilent 720ES).

[0114] The infrared high reflection layer is an ITO film, whose visible light transmittance of 400-760nm is 87%, and the infrared reflectivity of 2.5-14μm is 86%.

[0115] The electrolyte layer was a 1 mol solution of lithium bis(trifluoromethanesulfonyl)imide in tetraethylene glycol dimethyl ether.

[0116] The ion storage layer is a platinum nanocrystal layer.

[0117] The counter electrode layer is a carbon nanotube film, which is opaque and has a resistance of 10Ω / sq.

[0118] The prepared novel electrovariable infrared emissivity device is an opaque device.

[0119] Performance Testing

[0120] (1) LSPR absorption peak detection of aluminum-doped zinc oxide nanocrystal dispersion

[0121] The LSPR absorption peak of the aluminum-doped zinc oxide nanocrystal dispersion prepared in Example 1 was detected by the following method:

[0122] A small amount of aluminum-doped zinc oxide nanocrystal dispersion is dropped into the slit between two BaF2 substrates, and the absorption peak of the aluminum-doped zinc oxide nanocrystals is tested in an infrared spectrometer, which is the LSPR absorption peak of the aluminum-doped zinc oxide nanocrystals.

[0123] The LSPR absorption peak detection results of the aluminum-doped zinc oxide nanocrystal dispersion prepared in Example 1-2 are as follows: Figure 2 As shown, Figure 2 The LSPR absorption peak of a is located at 3.15nm. Figure 2 The LSPR absorption peak of b is located at 7.78 μm.

[0124] (2) Surface morphology detection of aluminum-doped zinc oxide nanocrystals

[0125] The surface morphology of the AZO nanocrystalline film was detected using a scanning electron microscope (FE-SEM; TESCAN MIRA). Figure 3 As shown, Figure 3a and 3b are the transmission electron microscope morphology and magnified images of AZO nanocrystals. Figure 3 c is the diameter distribution diagram of AZO nanocrystals. It can be seen from the figure that the diameter of AZO nanocrystals is in the range of 2-16nm.

[0126] (3) Cross-sectional morphology detection of BaF2 / AZO nanocrystal film / ITO film semi-device

[0127] The cross-sectional morphology was examined using TEM (FEI Talos F200s) and energy dispersive spectroscopy (EDS; super-X). Figure 4 described.

[0128] (4) Spectral detection of visible light and infrared emissivity control of electro-variable infrared emissivity devices

[0129] The visible light spectrum detection and infrared emissivity regulation detection of the electrovariable infrared emissivity device prepared in Example 1 are performed as follows: an ultraviolet visible near infrared (UV-Vis-NIR) spectrophotometer is used to test the spectral changes of visible light of the electrovariable infrared emissivity device, and a Fourier transform infrared spectrometer (FTIR) is used to test the infrared spectrum of the electrovariable infrared emissivity device.

[0130] Test results such as Figure 5 As shown by Figure 5 It can be seen that the regulation amount of the infrared band of 3 to 5 μm is 0.51, the regulation amount of the infrared emissivity of 8 to 14 μm is 0.42, and the transmittance of visible light is 84.7%.

[0131] The infrared spectrum of the electro-variable infrared emissivity device prepared in Example 2 was tested and the results were as follows: Figure 6 As shown by Figure 6 It can be seen that the control amount of the infrared band of 3 to 5 μm is 0.1, and the control amount of the infrared emissivity of 8 to 14 μm is 0.1.

[0132] (5) Fast response time detection of electro-variable infrared emissivity devices

[0133] The detection method is to use an infrared thermal imager to record the change in apparent temperature of the electrotropic infrared emissivity device after positive and negative voltages are applied. The time taken to reach 90% of the maximum apparent temperature after the voltage is applied is defined as the response time of the electrotropic infrared emissivity device.

[0134] Test results such as Figure 7 As shown, from Figure 7 It can be seen that the fast response time of the electrotropic infrared emissivity device is less than 600ms, and the apparent temperature change is greater than 6°C.

[0135] (6) Cyclic performance test of electro-variable infrared emissivity devices

[0136] The detection method is to use an electrochemical workstation to test the cycle performance of the electrotropic infrared emissivity device through multiple positive and negative voltage cycles. The maximum apparent temperature difference between the positive and negative voltages is recorded using an infrared thermal imager to determine whether the device has failed. The maximum apparent temperature difference of the device shows a significant decrease as the basis for judgment.

[0137] Test results such as Figure 8 As shown, from Figure 8 It can be seen that the cyclability of the electrotropic infrared emissivity device is greater than 10,000 times.

[0138] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.

Claims

1. A novel electro-variable infrared emissivity device, characterized in that: The electro-variable infrared emissivity device comprises, from top to bottom, an infrared transparent substrate layer, a variable infrared emissivity functional layer, an infrared high reflective layer, an electrolyte layer, an ion storage layer and a counter electrode layer; the infrared high reflective layer and the counter electrode layer are connected to the positive and negative electrodes, respectively; the variable infrared emissivity functional layer is doped zinc oxide nanocrystals, the doped ions in the doped zinc oxide nanocrystals are trivalent metal ions, the doping amount of the trivalent metal ions is 0.1-10%, and the infrared high reflective layer is selected from one of a metal film, an ITO film, an AZO film, a FTO film, and a Mxene film; The localized surface plasmon resonance absorption peak of the doped zinc oxide nanocrystal is located in the 3-14 μm infrared band. The localized surface plasmon resonance absorption peak is enhanced and weakened by electrochemical injection and extraction of electrons, thereby achieving regulation of the infrared emissivity of the doped zinc oxide nanocrystal.

2. The novel electrovariable infrared emissivity device according to claim 1, characterized in that: The diameter of the doped zinc oxide nanocrystal is 2-30 nm.

3. The novel electro-variable infrared emissivity device according to claim 1, characterized in that: The control amount of the electrovariable infrared emissivity device for the infrared band of 3 to 5 μm is 0.1 to 0.6, and the control amount of the infrared emissivity for 8 to 14 μm is 0.1 to 0.

6.

4. The novel electrovariable infrared emissivity device according to claim 1, characterized in that: The trivalent metal ion is one of aluminum ion, boron ion, gallium ion or indium ion.

5. The novel electro-variable infrared emissivity device according to claim 1, characterized in that: The material of the infrared transparent substrate layer is selected from one of BaF2, CaF2, polypropylene, polyethylene, polytetrafluoroethylene, nylon or silicon wafer, and the thickness of the variable infrared emissivity functional layer is 0.1-10 μm.

6. The novel electro-variable infrared emissivity device according to claim 1, characterized in that: The ion storage layer is one of a Pt nanocrystalline layer, an AZO film, a NiO film, and a V2O5 film.

7. The novel electro-variable infrared emissivity device according to claim 1, characterized in that: The counter electrode layer is selected from one of ITO glass, AZO glass, ITO flexible film, AZO flexible film, carbon nanotube film, metal grid glass or metal substrate.

8. The method for preparing the novel electrovariable infrared emissivity device according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Preparation of upper layer semi-device: Select an infrared transparent substrate material, spin-coat a doped zinc oxide nanocrystal dispersion with a trivalent metal ion doping amount of 0.1 to 10% onto the infrared transparent substrate material until the doped zinc oxide nanocrystal has a thickness of 0.1 to 10 μm, then evaporate a layer of thin film material on the upper surface of the doped zinc oxide nanocrystal as an infrared high reflection layer, lead electrode leads from the infrared high reflection layer thin film, and prepare an upper semiconductor device; S2. Preparation of lower layer semi-device: Selecting a counter electrode layer material, spin-coating a dispersion for ion storage onto the counter electrode layer material, and leading an electrode lead from the counter electrode layer to prepare a lower layer semi-device; S3. Preparation of new electro-variable infrared emissivity device: The upper half device prepared in S1 and the lower half device prepared in S2 are bonded together by transparent silicone rubber, and an electrolyte solution is injected into the middle to obtain a novel electrovariable infrared emissivity device.

9. The method for preparing the novel electrovariable infrared emissivity device according to claim 8, characterized in that: In step S1, after the doped zinc oxide nanocrystal dispersion is spin-coated onto the infrared transparent substrate layer material, the infrared transparent substrate / doped zinc oxide nanocrystal is heated in an argon environment at 250° C. for 30 minutes.

Citation Information

Patent Citations

  • Colloidal infrared reflective and transparent conductive aluminum-doped zinc oxide nanocrystals

    CN103370440A