Catalyst for catalyzing ammonia nitrogen into nitrite nitrogen, preparation method, application and preparation device

Through the reaction of Fe2+ and Mn2+ solutions with oxidants and complexing agents, a catalyst is generated under alkaline conditions, which solves the problems of low catalyst preparation efficiency and harsh conditions in the existing technology, and achieves efficient catalysis of ammonia nitrogen into sub-substrates at normal temperatures and pressures. The effect of nitrate nitrogen is suitable for industrial applications.

CN116440921BActive Publication Date: 2024-10-15BEIJING ORIGIN WATER FILM TECH
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202211675478.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-10-15
Estimated Expiration
2042-12-26

Smart Images

  • Figure CN116440921B_ABST
    Figure CN116440921B_ABST
Patent Text Reader

Abstract

The present invention provides a catalyst for catalyzing ammonia nitrogen to nitrite nitrogen, a preparation method, an application and a preparation device. The preparation method comprises the following steps: preparing Fe 2+ With Mn 2+ solution, an oxidant solution; the oxidant solution comprises an oxidant and a pH adjuster, wherein the pH of the oxidant solution is 8-9; Fe 2+ With Mn 2+ The solution is contacted with an oxidant solution to undergo a redox reaction to obtain an iron-manganese oxide; the iron-manganese oxide is contacted with a complexing agent solution to undergo a complexing reaction to obtain an iron-manganese complex solution, wherein the iron-manganese complex contains a trivalent manganese complex, a divalent iron complex, and a trivalent iron complex; an alkaline solution is added to the iron-manganese complex solution to undergo a disproportionation reaction to generate a precipitate, and the precipitate is separated to obtain a catalyst for catalyzing ammonia nitrogen to nitrite nitrogen. The catalyst can catalyze the oxidation of ammonia nitrogen to nitrite nitrogen at normal temperature and pressure, and the preparation process is simple and fast, with low cost, and is conducive to industrial scale-up.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalytic oxidation treatment of ammonia nitrogen, and specifically relates to a catalyst for catalyzing ammonia nitrogen into nitrite nitrogen, a preparation method, an application and a preparation device. Background Art

[0002] Ammonia nitrogen in municipal water is mainly in the form of ammonium ions (NH4 + ) exists in the form of catalytic oxidation treatment of ammonia nitrogen in actual municipal water bodies polluted by low concentrations of ammonia nitrogen. The main methods currently used are contact catalytic oxidation (for example, the publication number is CN110508289 A, and the patent name is a Chinese patent for an active filter material preparation system for catalytic oxidation removal of iron, manganese and ammonia nitrogen in water) and wet catalytic oxidation (for example, the publication number is CN 109465008 A, and the patent name is a Chinese patent for a catalytic wet oxidation catalyst and its preparation method and application).

[0003] The contact catalytic oxidation method is specifically: using potassium permanganate and Mn 2+ and Fe 2+ Reaction, Mn 2+ and Fe 2+ The iron-manganese oxides generated by potassium permanganate oxidation are retained on the surface of the quartz sand and gradually form a layer that is not easy to fall off and has the function of catalyzing the oxidation of NH4 + The iron-manganese oxide film is produced by the method, but the preparation method has the following disadvantages: 1. The catalyst preparation efficiency is low and the cycle is long, which is 1-4 months; 2. The catalyst preparation system includes a film-forming water tank, a static mixer, a reagent dosing system, a preparation main body system, a forward low-flow rate film-forming circulation loop, a forward high-flow rate film-forming circulation loop and a reverse low-flow rate film-forming circulation loop, and regular air-water backwashing is required, which has high energy consumption and complicated operation.

[0004] Wet catalytic oxidation technology is an advanced oxidation technology that uses air or oxygen as an oxidant in a high temperature (120-374°C) and high pressure (0.5-20MPa) environment to oxidize dissolved or suspended organic matter and reduce inorganic matter in water. Although wet catalytic oxidation technology has good ammonia nitrogen treatment effect, its reaction conditions are harsh, requiring high temperature, high pressure, and high pH (pH>10), high equipment costs, and catalysts mostly use precious metals, which have high preparation costs. There are still great difficulties in actual promotion and application. Summary of the invention

[0005] The present invention aims to solve the problems of low preparation efficiency, long cycle and complicated preparation process of ammonium catalyst prepared by contact biofilm method in catalytic oxidation treatment method of ammonia nitrogen, and the problem that a series of harsh conditions such as high temperature, high pressure and high pH are required in wet catalytic oxidation method. A catalyst for catalyzing ammonia nitrogen to nitrite nitrogen, a preparation method, application and preparation device are provided. The catalyst can catalytically oxidize ammonia nitrogen to nitrite nitrogen under normal temperature and pressure conditions, and the preparation process is simple and fast, the cost is low, and it is conducive to industrial scale-up.

[0006] In order to solve the above problems, the first aspect of the present invention provides a method for preparing a catalyst for catalyzing ammonia nitrogen to nitrite nitrogen, comprising the following steps:

[0007] S001. Preparation of Fe 2+ With Mn 2+ solution, an oxidant solution; the oxidant solution comprises an oxidant and a pH adjuster, and the pH adjuster makes the pH of the oxidant solution be 8-9;

[0008] S002. The Fe 2+ With Mn 2+ The solution is contacted with the oxidant solution to undergo an oxidation-reduction reaction to obtain iron-manganese oxides, wherein the iron-manganese oxides include trivalent manganese oxides, divalent iron oxides, and trivalent iron oxides;

[0009] S003. contacting the iron-manganese oxide with a complexing agent solution to perform a complexing reaction to obtain an iron-manganese complex solution, wherein the iron-manganese complex comprises a trivalent manganese complex, a divalent iron complex, and a trivalent iron complex;

[0010] S004. Adding an alkaline solution to the iron-manganese complex solution to carry out a disproportionation reaction to generate a precipitate, and separating the precipitate to obtain the catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

[0011] Preferably, the oxidant is at least one of potassium permanganate, potassium persulfate, sodium permanganate, and sodium persulfate;

[0012] The pH regulator is at least one of sodium bicarbonate, sodium hydroxide and potassium hydroxide;

[0013] The complexing agent is at least one of sodium pyrophosphate, deferoxamine trihydroxamate, and ethylenediaminetetraacetic acid;

[0014] The alkaline solution is at least one of a sodium hydroxide solution and a potassium hydroxide solution.

[0015] Preferably, the Fe 2+ With Mn 2+ In solution, Fe 2+ The concentration is 1-10 mmol / L, Mn 2+Concentration is 4-40 mmol / L;

[0016] In the oxidant solution, the concentration of the oxidant is 1.4-30 mmol / L, and the concentration of the pH adjuster is 2-30 mmol / L;

[0017] In the complexing agent solution, the concentration of the complexing agent is 10-50 g / L;

[0018] The concentration of the alkaline solution is 0.5-1 mol / L.

[0019] Preferably, in step S002, the Fe 2+ With Mn 2+ The volume ratio of the solution to the oxidant solution is (0.9-2):1;

[0020] In step S003, the mass ratio of the iron-manganese oxide to the complexing agent is 1:(1-2).

[0021] Preferably, in step S001, Fe 2+ With Mn 2+ solution, also adjust the Fe 2+ With Mn 2+ The pH of the solution is 2.7-3.5.

[0022] Preferably, step S003 specifically comprises: mixing the iron-manganese oxide with the complexing agent solution, stirring for reaction, and then standing for 8-12 hours, and after the solid is completely precipitated, filtering to obtain a solution, which is the iron-manganese complex solution.

[0023] Preferably, step S004 is specifically as follows: adding an alkaline solution to the iron-manganese complex solution while continuously stirring until an obvious precipitate is generated and the supernatant is colorless, stopping the addition of the alkaline solution, and then continuing to stir for 3-6 hours, stopping stirring, standing and aging for 12-24 hours, then filtering, washing to neutrality, separating the precipitate, and obtaining the catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

[0024] The second aspect of the present invention provides a catalyst for converting ammonia nitrogen into nitrite nitrogen prepared by the above-mentioned preparation method.

[0025] In a third aspect of the present invention, the catalyst for converting ammonia nitrogen into nitrite nitrogen is used for catalytically oxidizing ammonia nitrogen into nitrite nitrogen.

[0026] A fourth aspect of the present invention provides a device for preparing a catalyst for converting ammonia nitrogen into nitrite nitrogen, comprising:

[0027] Fe 2+ With Mn 2+ Solution supply device for providing Fe 2+With Mn 2+ Solution;

[0028] An oxidant solution supply device, used for providing an oxidant solution, wherein the oxidant solution includes an oxidant and a pH adjuster;

[0029] A tee, one inlet of the tee is connected to the Fe 2+ With Mn 2+ The outlet of the solution supply device is connected, and the other inlet of the tee is connected to the outlet of the oxidant solution supply device;

[0030] A mixer, the inlet of the mixer is connected to the outlet of the tee;

[0031] An iron-manganese oxide storage device is connected to the outlet of the mixer and is used to store the iron-manganese oxide and to allow the iron-manganese oxide to contact with the complexing agent for complexing reaction;

[0032] An iron-manganese complex separation device is used to separate the solid-liquid product obtained from the complex reaction to obtain an iron-manganese complex solution;

[0033] An iron-manganese complex disproportionation reaction device is used for the iron-manganese complex to contact with an alkaline solution for disproportionation reaction;

[0034] The disproportionation product separation device is used to separate the solid and liquid products obtained from the disproportionation reaction to obtain a catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The catalyst for catalyzing ammonia nitrogen to nitrite nitrogen of the present invention can catalyze the oxidation of ammonia nitrogen to nitrite nitrogen under normal temperature and pressure conditions, has a simple and rapid preparation process, is low in cost, and is conducive to industrial scale-up.

[0037] The preparation method of the catalyst for catalyzing ammonia nitrogen to nitrite nitrogen of the present invention, Fe 2+ With Mn 2+ The solution and the oxidant undergo a redox reaction under alkaline conditions to generate an iron-manganese oxide containing trivalent manganese oxide, divalent iron oxide and trivalent iron oxide, and then the iron-manganese oxide reacts with a complexing agent to generate a soluble trivalent manganese complex, a divalent iron complex and a trivalent iron complex to obtain dissolved trivalent manganese, divalent iron and trivalent iron, and then a disproportionation reaction is carried out to obtain an iron-manganese oxide with a catalytic effect, wherein the main components of the iron-manganese oxide are delta-MnO2 and FeOOH, and the catalyst can catalytically oxidize ammonia nitrogen to nitrite nitrogen under normal temperature and pressure conditions, and the preparation process is simple and rapid, the cost is low, and it is conducive to industrial scale-up. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1It is a schematic structural diagram of a device for preparing a catalyst for converting ammonia nitrogen into nitrite nitrogen according to Example 1 of the present invention;

[0039] Figure 2 is a SEM image of the catalyst prepared in Example 2 of the present invention;

[0040] Figure 3 is the XRD pattern of the catalyst prepared in Example 2 of the present invention;

[0041] Figure 4 is a SEM image of the catalyst prepared in Example 3 of the present invention;

[0042] Figure 5 This is the XRD diagram of the catalyst prepared in Example 3 of the present invention.

[0043] Among them: 1-Fe 2+ , Mn 2+ Solution storage tank; 2-oxidant solution storage tank; 3-iron-manganese oxide storage tank; 4-peristaltic pump; 5-peristaltic pump; 6-ball valve; 7-ball valve; 8-Y-type three-way; 9-static mixer; 10-iron-manganese complex filter; 11-disproportionate product filter. DETAILED DESCRIPTION

[0044] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] In the catalytic oxidation treatment method of ammonia nitrogen in actual municipal water bodies polluted by low concentrations of ammonia nitrogen, the contact catalytic oxidation method is used to prepare the ammonium catalyst, which has a long cycle, low yield, and a complex preparation system. The wet catalytic oxidation method has harsh reaction conditions and requires high temperature, high pressure, and high pH (pH>10), high equipment costs, and the catalyst mostly uses precious metals, which has a high preparation cost.

[0046] To this end, a first aspect of an embodiment of the present invention provides a method for preparing a catalyst for converting ammonia nitrogen into nitrite nitrogen, comprising the following steps:

[0047] S001. Preparation of Fe 2+ With Mn 2+ solution, an oxidant solution; the oxidant solution comprises an oxidant and a pH adjuster, and the pH adjuster makes the pH of the oxidant solution be 8-9;

[0048] S002. The Fe 2+ With Mn 2+The solution is contacted with the oxidant solution to undergo an oxidation-reduction reaction to obtain iron-manganese oxides, wherein the iron-manganese oxides include trivalent manganese oxides, divalent iron oxides, and trivalent iron oxides;

[0049] S003. contacting the iron-manganese oxide with a complexing agent solution to perform a complexing reaction to obtain an iron-manganese complex solution, wherein the iron-manganese complex comprises a trivalent manganese complex, a divalent iron complex, and a trivalent iron complex;

[0050] S004. Adding an alkaline solution to the iron-manganese complex solution to carry out a disproportionation reaction to generate a precipitate, and separating the precipitate to obtain the catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

[0051] Preparation method of the catalyst for catalyzing ammonia nitrogen to nitrite nitrogen according to the embodiment of the present invention, Fe 2+ With Mn 2+ The solution and the oxidant undergo a redox reaction under alkaline conditions to generate an iron-manganese oxide containing trivalent manganese oxide, divalent iron oxide and trivalent iron oxide, and then the iron-manganese oxide reacts with a complexing agent to generate a soluble trivalent manganese complex, a divalent iron complex and a trivalent iron complex to obtain dissolved trivalent manganese, divalent iron and trivalent iron, and then a disproportionation reaction is carried out to obtain an iron-manganese oxide with a catalytic effect, wherein the main components of the iron-manganese oxide are delta-MnO2 and FeOOH, and the catalyst can catalytically oxidize ammonia nitrogen to nitrite nitrogen under normal temperature and pressure conditions, and the preparation process is simple and rapid, the cost is low, and it is conducive to industrial scale-up.

[0052] In some embodiments, Fe 2+ With Mn 2+ The solution can be Fe 2+ , Mn 2+ The inorganic salt or organic salt thereof may be, for example, sulfate, hydrochloride, nitrate, etc., and the organic salt may be acetate, sulfonate, etc. 2+ With Mn 2+ The solution may be an aqueous solution.

[0053] In some embodiments, the oxidant acts to convert Fe 2+ , Mn 2+ Oxidized to oxides, the oxidant is preferably a strong oxidant, wherein the strong oxidant can be at least one of potassium permanganate, potassium persulfate, sodium permanganate, and sodium persulfate. Preferably, the oxidant is potassium permanganate.

[0054] In some embodiments, the pH adjuster is used to make the pH of the oxidant solution alkaline, ensuring that Fe 2+ With Mn 2+The pH regulator can be at least one of sodium bicarbonate, sodium hydroxide, and potassium hydroxide. Preferably, the pH regulator is sodium bicarbonate.

[0055] In some embodiments, the oxidant solution may be an aqueous solution of an oxidant and a pH adjuster.

[0056] In some embodiments, the function of the complexing agent is to react with iron-manganese oxide to generate soluble trivalent manganese complex, divalent iron complex, and trivalent iron complex. The complexing agent can be at least one of sodium pyrophosphate, triisohydroxamic acid deferoxamine, and ethylenediaminetetraacetic acid. Preferably, the complexing agent is sodium pyrophosphate.

[0057] In some embodiments, the alkaline solution is used to cause disproportionation reaction of soluble trivalent manganese and trivalent iron. The alkaline solution can be at least one of a sodium hydroxide solution and a potassium hydroxide solution.

[0058] In some embodiments, Fe 2+ With Mn 2+ In solution, Fe 2+ With Mn 2+ Fe 2+ The concentration of Fe is not limited, preferably, 2+ The concentration is 1-10 mmol / L, Mn 2+ The concentration is 4-40 mmol / L. The iron-manganese oxide synthesized with a concentration in this range can enable the next step of complexation reaction to obtain a complex solution containing trivalent manganese with a higher concentration.

[0059] In some embodiments, the concentrations of the oxidant and the pH adjuster in the oxidant solution are not limited, preferably, the concentration of the oxidant is 1.4-30 mmol / L, and the concentration of the pH adjuster is 2-30 mmol / L. The iron-manganese oxide synthesized with a concentration in this range can allow the next step of the complex reaction to obtain a higher concentration of trivalent manganese-containing complex solution.

[0060] In some embodiments, in the complexing agent solution, the concentration of the complexing agent is not particularly limited. Preferably, the concentration of the complexing agent is 10-50 g / L.

[0061] In some embodiments, the concentration of the alkaline solution is not particularly limited, and preferably, the concentration of the alkaline solution is 0.5-1 mol / L. When the concentration is within this range, the disproportionation effect is fastest and best, and excessive disproportionation can be prevented.

[0062] In some embodiments, in step S002, Fe 2+ With Mn 2+ The volume ratio of Fe solution to oxidant solution is not particularly limited. Preferably, Fe 2+With Mn 2+ The volume ratio of the solution to the oxidant solution is (0.9-2): 1. The iron-manganese oxide obtained by the reaction using this volume ratio is most suitable for the next step of complex reaction to obtain a trivalent manganese complex solution.

[0063] In some embodiments, in step S003, the mass ratio of iron-manganese oxide to complexing agent is not particularly limited, preferably, the mass ratio of iron-manganese oxide to complexing agent is 1:(1-2). Thus, the complexing reaction effect is the best, the complexing agent is saved the most, and it is also conducive to the next step of rapid disproportionation.

[0064] In some embodiments, in step S001, Fe 2+ With Mn 2+ When the solution is adjusted, Fe 2+ With Mn 2+ The pH of the solution is 2.7-3.5. This can prevent Fe 2+ , Mn 2+ Hydrolysis and oxidation.

[0065] In some embodiments, in step S002, Fe 2+ With Mn 2+ The specific method of contacting the solution with the oxidant solution is not limited. For example, Fe 2+ With Mn 2+ solution and oxidant solution, and then mix the two solutions; Fe 2+ With Mn 2+ solution, add oxidant and pH adjuster to Fe 2+ With Mn 2+ solution and mix them; you can also prepare an oxidant solution and then 2+ Salt and Mn 2+ The salt is dissolved in the oxidant solution and allowed to mix.

[0066] In some embodiments, in step S003, the specific method of contacting the iron manganese oxide with the complexing agent solution is not limited. For example, the complexing agent can be added to the dispersion of the iron manganese oxide product reacted in step S002, so that the complexing agent is dissolved in the solvent in the dispersion, and the two are mixed; or the complexing agent solution can be prepared first, and the complexing agent solution is added to the dispersion of the iron manganese oxide product reacted in step S002, and the two are mixed; or the complexing agent solution can be prepared, and the iron manganese oxide is added to the complexing agent solution, and the two are mixed.

[0067] In some embodiments, in step S003, the reaction time of the complexing reaction is not particularly limited. Preferably, the iron-manganese oxide is mixed with the complexing agent solution, stirred for reaction, and then left to stand for 8-12 hours.

[0068] In some embodiments, step S003 also includes a separation step of the iron-manganese complex, and the specific separation method is not limited, as long as the iron-manganese complex can be separated from other solids. Preferably, the iron-manganese complex is separated by filtration, and after the solid is completely settled, a solution is obtained by suction filtration, which is the iron-manganese complex solution.

[0069] In some embodiments, in step S004, an alkaline solution is added to the iron-manganese complex solution. The method is not particularly limited. For example, an alkaline compound can be added to the iron-manganese complex solution to dissolve it, thereby causing the iron-manganese complex to undergo a disproportionation reaction. The alkaline compound can also be prepared into a solution, and the alkaline solution is added to the iron-manganese complex solution for a disproportionation reaction.

[0070] In some embodiments, the reaction time of the disproportionation reaction is not particularly limited. Preferably, an alkaline solution is added to the iron-manganese complex solution while stirring continuously until an obvious precipitate is generated and the supernatant is colorless, then the addition of the alkaline solution is stopped, and the stirring reaction is continued for 3-6 hours.

[0071] In some embodiments, step S004 further includes an aging step for the disproportionation reaction product. Preferably, the disproportionation reaction product is aged for 12-24 hours. Thus, the product crystal structure can be more stable and complete.

[0072] In some embodiments, step S004 further includes a step of separating the disproportionation reaction product. The specific operation mode of separation is not particularly limited, and preferably, the product after the disproportionation reaction and aging is filtered, washed to neutrality, and separated to precipitate.

[0073] A second aspect of an embodiment of the present invention provides a catalyst for converting ammonia nitrogen into nitrite nitrogen prepared by the above-mentioned preparation method.

[0074] The catalyst for converting ammonia nitrogen to nitrite nitrogen in the embodiment of the present invention can catalyze the oxidation of ammonia nitrogen to nitrite nitrogen under normal temperature and pressure conditions. The preparation process is simple and fast, the cost is low, and it is conducive to industrial scale-up. In addition, the catalyst has a large specific surface area and has very good deammoniation performance.

[0075] A third aspect of an embodiment of the present invention is an application of the above-mentioned catalyst for catalyzing the conversion of ammonia nitrogen into nitrite nitrogen, which is used for catalytic oxidation of ammonia nitrogen into nitrite nitrogen.

[0076] A fourth aspect of an embodiment of the present invention provides a device for preparing a catalyst for converting ammonia nitrogen into nitrite nitrogen, comprising:

[0077] Fe 2+ With Mn 2+ Solution supply device for providing Fe 2+ With Mn 2+Solution;

[0078] An oxidant solution supply device, used for providing an oxidant solution, wherein the oxidant solution includes an oxidant and a pH adjuster;

[0079] A tee, one inlet of the tee is connected to the Fe 2+ With Mn 2+ The outlet of the solution supply device is connected, and the other inlet of the tee is connected to the outlet of the oxidant solution supply device;

[0080] A mixer, the inlet of the mixer is connected to the outlet of the tee;

[0081] An iron-manganese oxide storage device is connected to the outlet of the mixer and is used to store the iron-manganese oxide and to allow the iron-manganese oxide to contact with the complexing agent for complexing reaction;

[0082] An iron-manganese complex separation device is used to separate the solid-liquid product obtained from the complex reaction to obtain an iron-manganese complex solution;

[0083] An iron-manganese complex disproportionation reaction device is used for the iron-manganese complex to contact with an alkaline solution for disproportionation reaction;

[0084] The disproportionation product separation device is used to separate the solid and liquid products obtained from the disproportionation reaction to obtain a catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

[0085] The preparation device of the catalyst for catalyzing ammonia nitrogen to nitrite nitrogen in the embodiment of the present invention can be used to prepare the above-mentioned catalyst for catalyzing ammonia nitrogen to nitrite nitrogen. The prepared catalyst can catalyze the oxidation of ammonia nitrogen to nitrite nitrogen under normal temperature and pressure conditions. The preparation process is simple, fast and low-cost.

[0086] In some embodiments, Fe 2+ With Mn 2+ The specific structure of the solution supply device is not limited, as long as it can quantitatively supply Fe 2+ With Mn 2+ Preferably, Fe 2+ With Mn 2+ The solution supply device includes Fe 2+ With Mn 2+ Solution storage tank and first peristaltic pump, Fe 2+ With Mn 2+ The outlet of the solution storage tank is connected to the first peristaltic pump.

[0087] In some embodiments, the specific structure of the oxidant solution supply device is not limited, as long as the oxidant solution can be quantitatively supplied. Preferably, the oxidant solution supply device includes an oxidant solution storage tank and a second peristaltic pump, and the outlet of the oxidant solution storage tank is connected to the second peristaltic pump.

[0088] In some embodiments, the specific structure of the mixer is not limited. Preferably, the mixer is a static mixer.

[0089] In some embodiments, the specific structure of the iron-manganese oxide storage device is not limited. Preferably, the iron-manganese oxide storage device is an iron-manganese oxide storage tank.

[0090] In some embodiments, the specific structure of the iron-manganese complex separation device is not limited, as long as it can separate the solid and the liquid, for example, it can be a filtering device.

[0091] In some embodiments, the specific structure of the iron-manganese complex disproportionation reaction device is not limited, as long as it can accommodate the iron-manganese complex for reaction. For example, the disproportionation reaction can be directly carried out in the iron-manganese oxide storage tank.

[0092] In some embodiments, the specific structure of the disproportionation product separation device is not limited, as long as it can separate the solid and the liquid, for example, it can be a filtering device.

[0093] Example

[0094] The raw materials used in the following examples were all purchased from commercial sources.

[0095] Example 1

[0096] like Figure 1 As shown, the preparation device of the catalyst for catalyzing ammonia nitrogen to nitrite nitrogen in this embodiment includes:

[0097] Fe 2+ , Mn 2+ Solution storage tank 1, used to store Fe 2+ With Mn 2+ Solution;

[0098] Peristaltic pump 4, with Fe 2+ , Mn 2+ The outlet connection of the solution storage tank 1;

[0099] An oxidant solution storage tank 2, used for storing the oxidant solution;

[0100] A peristaltic pump 5 is connected to the outlet of the oxidant solution storage tank 2;

[0101] Y-type tee 8, one inlet and Fe 2+ , Mn 2+ The outlet of the solution storage tank 1 is connected, and the other inlet is connected to the outlet of the oxidant solution storage tank 2;

[0102] The ball valve 6 is provided between the interface of the peristaltic pump 4 and the Y-type tee 8; the ball valve 7 is provided between the interface of the peristaltic pump 5 and the Y-type tee 8;

[0103] A static mixer 9, the inlet of the static mixer 9 is connected to the outlet of the Y-shaped tee 8;

[0104] The iron-manganese oxide storage tank 3 is connected to the outlet of the static mixer 9 and is used to store the iron-manganese oxide and to contact the iron-manganese oxide with the complexing agent for complexing reaction;

[0105] The iron-manganese complex filter 10 is used to separate the iron-manganese complex; the disproportionation product filter 11 is used to separate the disproportionation reaction products.

[0106] Example 2

[0107] The preparation method of the catalyst for catalyzing ammonia nitrogen to nitrite nitrogen in this embodiment comprises the following steps:

[0108] S001. Preparation of Fe 2+ , Mn 2+ Solution 20L, Fe 2+ The concentration is 5 mmol / L, Mn 2+ The concentration is 25 mmol / L, and the pH of the solution is adjusted to 2.7-3.5 to prevent Fe 2+ , Mn 2+ Hydrolysis oxidation, the iron manganese salt used is sulfate; prepare 20L of potassium permanganate and sodium bicarbonate solution, the concentration of potassium permanganate is 19mmol / L, and the concentration of sodium bicarbonate is 25mmol / L;

[0109] S002. Open ball valve switches 6 and 7, and peristaltic pump 4 will pump Fe 2+ , Mn 2+ Fe in solution storage tank 1 2+ , Mn 2+ The solution is lifted to the Y-type tee 8 at a certain flow rate, and the peristaltic pump 5 lifts the potassium permanganate and sodium bicarbonate solutions in the potassium permanganate and sodium bicarbonate solution storage tank 2 to the Y-type tee 8 at the same flow rate (i.e., Fe 2+ With Mn 2+ The volume ratio of the solution to the oxidant solution was 1:1), the flow rate was 120 mL / min, and the Fe 2+ , Mn 2+ reacting with potassium permanganate at the Y-type tee, and the mixed solution after the reaction flows to the static mixer 9 for further mixing and sufficient reaction, and the reaction time is 2 minutes to obtain iron-manganese oxide, wherein the iron-manganese oxide contains trivalent manganese oxide, divalent iron oxide, and trivalent iron oxide, and then enters the iron-manganese oxide storage tank 3 for standby use;

[0110] S003. Adding solid sodium pyrophosphate to the iron-manganese oxide storage tank 3, so that the sodium pyrophosphate concentration is 25g / L, that is, the mass ratio of iron-manganese oxide to the complexing agent is 1:2, and then stirring for 5h to fully dissolve the sodium pyrophosphate, and then fully contacting with the iron-manganese oxide in the iron-manganese oxide storage tank to carry out a complex reaction, solid trivalent manganese in the iron-manganese oxide combines with sodium pyrophosphate to obtain soluble complexed trivalent manganese, and there are partially complexed divalent iron and trivalent iron. After the stirring is completed, let it stand for 12h, and after the solid is completely settled, filter to obtain a solution, that is, a dissolved trivalent manganese complex, a divalent iron complex, and a trivalent iron complex;

[0111] S004. Take 30L of the iron-manganese complex solution obtained above, slowly add 1mol / L sodium hydroxide solution thereto, and keep stirring until obvious precipitate is generated and the supernatant is colorless, then stop adding the sodium hydroxide solution, and continue stirring for 4h. After sufficient reaction, stop stirring, let stand and age for 24h, then filter and wash, and fully wash the material to neutrality to obtain a product, which is a catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

[0112] A portion of the catalyst material was dried at room temperature for 48 h and used for XRD and SEM characterization. Figure 2 and Figure 3 As shown, another 30 g of filter cake was taken for deammonium performance testing.

[0113] Depend on Figure 2 It can be seen that the catalyst surface presents a flaky and wrinkled structure, indicating that the catalyst has a large surface area, which is conducive to the adsorption of ammonia nitrogen.

[0114] Depend on Figure 3 It can be seen that there are three peaks in the XRD pattern, namely 18.24° 2θ, 36.52° 2θ, and 65.16° 2θ, of which 36.52° 2θ and 65.16° 2θ are characteristic peaks of δ-MnO2, and 18.24° 2θ is a characteristic peak of FeOOH. This indicates that the main components of the ammonium catalyst producing nitrite nitrogen are δ-MnO2 and FeOOH.

[0115] The deammonium performance is shown in Table 1. After 48 hours of stirring and aeration, the ammonia nitrogen concentration decreased from 41.79 mg / L to 0.12 mg / L. The ammonia nitrogen was completely catalytically oxidized, and the total nitrogen did not decrease. The oxidation product was nitrite nitrogen, which has very good deammonium performance. Nitrite nitrogen can accumulate continuously and stably.

[0116] Table 1 Ammonia nitrogen removal effect of municipal sewage in Beijing

[0117] Aeration time (h) Ammonia nitrogen (mg / L) Nitrate nitrogen (mg / L) Nitrite nitrogen (mg / L) Total nitrogen (mg / L) 0 41.79 3.22 0.003 44.7 3 37.62 3.15 3.28 44.83 18 23.12 3.36 19.5 45.02 26 12.33 3.14 30.5 44.46 48 0.12 3.25 41.25 44.44

[0118] Example 3

[0119] The preparation method of the catalyst for catalyzing ammonia nitrogen to nitrite nitrogen in this embodiment comprises the following steps:

[0120] S001. Preparation of Fe 2+ , Mn 2+ Solution 30L, Fe 2+ The concentration is 7 mmol / L, Mn 2+ The concentration is 10 mmol / L, and the solution pH is adjusted to 2.7-3.5 to prevent Fe 2+ , Mn 2+ Hydrolysis oxidation, the iron manganese salt used is hydrochloride; prepare 30L of potassium permanganate and sodium bicarbonate solution, the concentration of potassium permanganate is 23mmol / L, and the concentration of sodium bicarbonate is 28mmol / L;

[0121] S002. Open ball valve switches 6 and 7, and peristaltic pump 4 will pump Fe 2+ , Mn 2+ Fe in solution storage tank 1 2+ , Mn 2+ The solution is lifted to the Y-type tee 8 at a certain flow rate, and the peristaltic pump 5 lifts the potassium permanganate and sodium bicarbonate solutions in the potassium permanganate and sodium bicarbonate solution storage tank 2 to the Y-type tee 8 at the same flow rate (i.e., Fe 2+ With Mn 2+ The volume ratio of the solution to the oxidant solution was 1:1), the flow rate was 72 mL / min, and the Fe 2+ , Mn 2+ reacting with potassium permanganate at the Y-type tee, and the mixed solution after the reaction flows to the static mixer 9 for further mixing and sufficient reaction, and the reaction time is 2 minutes to obtain iron-manganese oxide, wherein the iron-manganese oxide contains trivalent manganese oxide, divalent iron oxide, and trivalent iron oxide, and then enters the iron-manganese oxide storage tank 3 for standby use;

[0122] S003. Adding solid sodium pyrophosphate to the iron-manganese oxide storage tank 3, so that the sodium pyrophosphate concentration is 10g / L, that is, the mass ratio of iron-manganese oxide to the complexing agent is 1:1, and then stirring for 3h to fully dissolve the sodium pyrophosphate, and then fully contacting with the iron-manganese oxide in the iron-manganese oxide storage tank to carry out a complex reaction, solid trivalent manganese in the iron-manganese oxide combines with sodium pyrophosphate to obtain soluble complexed trivalent manganese, and there are partially complexed divalent iron and trivalent iron. After the stirring is completed, let it stand for 12h, and after the solid is completely settled, filter to obtain a solution, that is, a dissolved trivalent manganese complex, a divalent iron complex, and a trivalent iron complex;

[0123] S004. Take 25L of the iron-manganese complex solution obtained above, slowly add 0.5mol / L sodium hydroxide solution thereto, and keep stirring until obvious precipitation is generated and the supernatant is colorless, then stop adding the sodium hydroxide solution, and continue stirring for 4h. After sufficient reaction, stop stirring, let stand and age for 18h, then filter and wash, and fully wash the material to neutrality to obtain a product, which is a catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

[0124] A portion of the catalyst material was dried at room temperature for 48 h and used for XRD and SEM characterization. Figure 4 and Figure 5 As shown, another 30 g of filter cake was taken for deammonium performance testing.

[0125] Depend on Figure 4 It can be seen that the catalyst surface presents a clustered flake-like, wrinkled porous structure. The catalyst synthesized at a low concentration has a larger surface area, which is more conducive to the adsorption of ammonia nitrogen.

[0126] Depend on Figure 5 It can be seen that there are four peaks in the XRD graph, namely 8.24° 2θ, 17.8° 2θ, 36.66° 2θ, and 65.3° 2θ, of which 8.24° 2θ, 36.52° 2θ, and 65.16° 2θ are characteristic peaks of δ-MnO2, and 17.8° 2θ is a characteristic peak of FeOOH. This indicates that the main components of the ammonium catalyst producing nitrite nitrogen are δ-MnO2 and FeOOH, and that the low-concentration synthetic catalyst δ-MnO2 has a higher crystal strength.

[0127] The deammonium performance is shown in Table 2. After 48 hours of stirring and aeration, the ammonia nitrogen concentration decreased from 30.56 mg / L to 0 mg / L. The ammonia nitrogen was completely catalytically oxidized, and the total nitrogen did not decrease. The oxidation product was nitrite nitrogen, which has very good deammonium performance. Nitrite nitrogen can accumulate continuously and stably.

[0128] Table 2 Ammonia nitrogen removal effect of municipal sewage in Beijing

[0129] Aeration time (h) Ammonia nitrogen (mg / L) Nitrate nitrogen (mg / L) Nitrite nitrogen (mg / L) Total nitrogen (mg / L) 0 30.56 5.47 0.013 36.22 5 25.96 5.33 3.28 35.93 18 13.02 5.46 18.25 36.42 26 0 5.32 30.27 35.95

[0130] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a catalyst for converting ammonia nitrogen into nitrite nitrogen, characterized in that: The following steps are involved: S001. Preparation of Fe 2+ With Mn 2+ solution, an oxidant solution; the oxidant solution comprises an oxidant and a pH adjuster, and the pH adjuster makes the pH of the oxidant solution be 8-9; S002. The Fe 2+ With Mn 2+ The solution is contacted with the oxidant solution to undergo an oxidation-reduction reaction to obtain iron-manganese oxides, wherein the iron-manganese oxides include trivalent manganese oxides, divalent iron oxides, and trivalent iron oxides; S003. contacting the iron-manganese oxide with a complexing agent solution to perform a complexing reaction to obtain an iron-manganese complex solution, wherein the iron-manganese complex comprises a trivalent manganese complex, a divalent iron complex, and a trivalent iron complex; S004. Adding an alkaline solution to the iron-manganese complex solution to carry out a disproportionation reaction to generate a precipitate, and separating the precipitate to obtain the catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

2. The preparation method according to claim 1, characterized in that: The oxidant is at least one of potassium permanganate, potassium persulfate, sodium permanganate and sodium persulfate; The pH regulator is at least one of sodium bicarbonate, sodium hydroxide and potassium hydroxide; The complexing agent is at least one of sodium pyrophosphate, deferoxamine trihydroxamate, and ethylenediaminetetraacetic acid; The alkaline solution is at least one of a sodium hydroxide solution and a potassium hydroxide solution.

3. The preparation method according to claim 1, characterized in that: The Fe 2+ With Mn 2+ In solution, Fe 2+ The concentration is 1-10mmol / L, Mn 2+ Concentration is 4-40mmol / L; In the oxidant solution, the concentration of the oxidant is 1.4-30 mmol / L, and the concentration of the pH adjuster is 2-30 mmol / L; In the complexing agent solution, the concentration of the complexing agent is 10-50 g / L; The concentration of the alkaline solution is 0.5-1 mol / L.

4. The preparation method according to claim 1, characterized in that: In step S002, the Fe 2+ With Mn 2+ The volume ratio of the solution to the oxidant solution is (0.9-2):1; In step S003, the mass ratio of the iron-manganese oxide to the complexing agent is 1:(1-2).

5. The preparation method according to claim 1, characterized in that: In step S001, Fe 2+ With Mn 2+ solution, also adjust the Fe 2+ With Mn 2+ The pH of the solution is 2.7-3.

5.

6. The preparation method according to claim 1, characterized in that: Step S003 specifically comprises: mixing the iron-manganese oxide with the complexing agent solution, stirring the mixture for reaction, and then standing the mixture for 8-12 hours. After the solid is completely precipitated, filtering the mixture to obtain a solution, which is the iron-manganese complex solution.

7. The preparation method according to claim 1, characterized in that: Step S004 is specifically as follows: adding an alkaline solution to the iron-manganese complex solution while continuously stirring until an obvious precipitate is generated and the supernatant is colorless, stopping the addition of the alkaline solution, and then continuing to stir for 3-6 hours, stopping stirring, standing and aging for 12-24 hours, then filtering, washing to neutrality, separating the precipitate, and obtaining the catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

8. A catalyst for converting ammonia nitrogen into nitrite nitrogen as prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the catalyst for catalyzing the conversion of ammonia nitrogen into nitrite nitrogen as claimed in claim 8, for catalytically oxidizing ammonia nitrogen into nitrite nitrogen.

10. A preparation device for a catalyst for converting ammonia nitrogen into nitrite nitrogen, characterized in that: include: Fe 2+ With Mn 2+ Solution supply device for providing Fe 2+ With Mn 2+ Solution; An oxidant solution supply device, used for providing an oxidant solution, wherein the oxidant solution includes an oxidant and a pH adjuster; A tee, one inlet of the tee is connected to the Fe 2+ With Mn 2+ The outlet of the solution supply device is connected, and the other inlet of the tee is connected to the outlet of the oxidant solution supply device; A mixer, the inlet of the mixer is connected to the outlet of the tee; An iron-manganese oxide storage device is connected to the outlet of the mixer and is used to store the iron-manganese oxide and to allow the iron-manganese oxide to contact with the complexing agent for complexing reaction; An iron-manganese complex separation device is used to separate the solid-liquid product obtained from the complex reaction to obtain an iron-manganese complex solution; An iron-manganese complex disproportionation reaction device is used for the iron-manganese complex to contact with an alkaline solution for disproportionation reaction; The disproportionation product separation device is used to separate the solid and liquid products obtained from the disproportionation reaction to obtain a catalyst that catalyzes ammonia nitrogen to nitrite nitrogen.

Citation Information

Patent Citations

  • Catalytic wet-type oxidation catalyst as well as preparation method and application thereof

    CN109465008A

  • Preparation system of active filter material for removing iron, manganese and ammonia nitrogen in water by catalytic oxidation

    CN110508289A

  • Hydrotalcite-like compound-spinel type ferrite combined material and preparation method thereof

    CN102430411A

  • Catalytic oxidation method for converting ferrous iron into ferric iron at normal temperature and normal pressure

    CN105731548A

  • Method for digesting manganese in manganese oxide ore through reduction with nitrosobacteria and dissolution and dilution with dilute acid

    CN107119188A