Flash gold dry particles made from slag and production method

By using low-cost materials such as apatite and slag and potassium dichromate solution, metallic gloss glass bodies are formed, which solves the problem of iron oxide utilization in slag, realizes the scintillation effect of flash gold dry particles, and reduces costs and environmental pollution. , improves the decorative effect of ceramic tiles.

CN116444163BActive Publication Date: 2024-11-26HUNAN TIANXIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310352164.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-11-26
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

The prior art is difficult to effectively use slag to make flash gold dry particles with metallic gloss effects, and there are problems of high cost and environmental pollution.

Method used

Using raw materials such as apatite, slag, zinc oxide, Jingyuan mud, sodafeldspar, glass powder and quartz, stirred and melted by potassium dichromate solution to form a glass body with metallic gloss crystals, which are quenched by water and broken into flash The gold dry particles use iron oxide and manganese dioxide in the slag to change the structure of the glass network to form crystals suspended in the glaze, achieving a scintillating metallic luster effect.

Benefits of technology

It reduces material costs, reduces environmental pollution, and forms golden, crystal-bright flashing dry particles, suitable for ceramic tiles surfaces, provides flashing effects similar to natural stone, and improves product grade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses flash gold dry particles made from slag, belonging to the field of building ceramic tiles. The raw materials include, by weight, 20-30 parts of apatite, 20-30 parts of slag, 3-8 parts of zinc oxide, 8-15 parts of Jingyuan mud, 10-15 parts of albite, 10-15 parts of glass powder and 5-12 parts of quartz. The invention also discloses a method for making the flash gold dry particles made from the slag, so that the dry particles have a flashing metallic luster effect, and the slag is reasonably used as a raw material for making the particles, which not only reduces environmental pollution but also greatly reduces the cost of the dry particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of building ceramic tiles, and in particular relates to flash gold dry particles made from slag and a production method thereof. Background Art

[0002] Building ceramic tiles are mainly easy to clean and decorative. Especially since the application and popularization of digital inkjet machines, the decoration method of building ceramic tiles basically relies on inkjet patterns to decorate the surface of ceramic tiles. Its decorative effect can imitate the surface texture and color of various materials in nature, especially the texture and color of natural marble, granite and wood. It is so vivid that it can be said that it is basically difficult to distinguish which is imitation stone ceramic tiles and which is real natural stone. The imitation technology has reached a level comparable to natural stone. Although the current building ceramic decoration technology can highly realistically restore the pattern texture and color of natural materials, the surface texture of some materials is difficult to imitate. For example, some natural stones will have naturally crystallized flashing particles. This texture will produce different directions of strong and weak reflections when observed from different angles, thus forming a flashing effect. The crystal particles in natural stone are natural. The natural crystals produced under the long-term geological action of marble generally run through the entire stone.

[0003] In order to get closer to the texture of natural stone, some natural or artificially prepared glittering granular materials are often added to the ceramic glaze during the production of ceramic tiles. They are fired at high temperatures together with the ceramic tile glaze in the hope of achieving this reflective glittering effect.

[0004] Introducing metallic luster effect in ceramic tiles will produce strong metallic luster with different lighting and viewing angles, giving people a visual shock and improving the grade of ceramic tile design. Metallic luster particles have a certain three-dimensional structure, which can bring better three-dimensional decorative effect. There are relatively few technologies for metallic luster particles in the prior art, which are mainly achieved by adding metal powder.

[0005] In recent years, with the rapid development of the domestic economy, the scale of mining in areas with mineral resources has increased, which inevitably causes huge pollution to the local environment. Slag is the waste slag produced when iron and steel plants smelt pig iron. Its open-air storage occupies land, pollutes and poisons the soil, water and atmosphere, seriously affects the ecological environment, and causes obvious or potential economic losses and waste of resources. In particular, the waste slag produced in the middle of smelting has an iron oxide content of more than 50%. Using slag to make particles with metallic luster and provide the required metal iron, titanium, manganese, vanadium, chromium, etc. can reduce costs and reduce pollution. However, the manganese dioxide contained in the slag is a modified body of the glass network structure, which can play a role in breaking the network, destroying the glass network structure composed of silicon dioxide and aluminum oxide, making the glass network structure loose. How to more reasonably use slag to make flash gold dry particles has become a technical problem that the present invention needs to solve. Summary of the invention

[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a flash gold dry granule made from slag and a production method, so that the dry granule has a flashing metallic luster effect, and reasonably utilizes slag and local inferior mud with high iron oxide content as production raw materials, which not only reduces environmental pollution, but also greatly reduces the cost of dry granules.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is:

[0008] A flash gold dry particle made from slag, wherein the raw materials include, by weight, 20-30 parts of apatite, 20-30 parts of slag, 3-8 parts of zinc oxide, 8-15 parts of Jingyuan mud, 10-15 parts of albite, 10-15 parts of glass powder and 5-12 parts of quartz.

[0009] Preferably, the raw materials include, by weight: 25 parts of apatite, 30 parts of slag, 3 parts of zinc oxide, 12 parts of Jingyuan mud, 15 parts of albite, 15 parts of glass powder, and 10 parts of quartz.

[0010] Furthermore, the chemical composition of the flash gold dry particles is: in mass percentage, SiO2 30-45%, Al2O3 5-10%, Fe2O3 10-13%, TiO2 0.5-1.4%, CaO 10-20%, MgO 0.5-1.7%, K2O 0.2-0.8%, Na2O 1.5-2.5%, ZnO 3-7%, MnO2 0.8-1.2%, Cr2O3 0.3-0.7%, V2O5 0.1-0.3%, P2O5 10-11%.

[0011] Preferably, the chemical composition of the flash gold dry particles is: in mass percentage, SiO2 40%, Al2O3 9%, Fe2O3 13%, TiO2 0.6%, CaO 15%, MgO 0.5%, K2O 0.5%, Na2O 2.5%, ZnO 7%, MnO2 1.2%, Cr2O3 0.4%, V2O5 0.3%, P2O5 10%.

[0012] A method for producing flash gold dry particles made from slag, characterized in that it comprises the following production steps:

[0013] Step 1: crush the raw materials of apatite, slag, zinc oxide, Jingyuan mud, albite, glass powder and quartz into 150-200 mesh powder, add potassium dichromate solution to the slag, mix and stir, and treat them separately, then weigh the raw material powders and the treated slag according to the above ratio and mix them, melt them, and finally quench them with water to obtain a glass body with metallic luster crystals;

[0014] Step 2: crush the glass obtained in step 1, and sieve to obtain the dry granules of golden chrysanthemum.

[0015] Furthermore, in step 1, the potassium dichromate solution is obtained by weighing 0.5-1% of the weight of the slag and dissolving it in water.

[0016] Furthermore, the melting temperature is 1200-1300°C.

[0017] Furthermore, after the melting, the temperature is cooled to 650-750° C. and kept at this temperature for 10 minutes.

[0018] Furthermore, the particle size of the prepared flash gold dry particles is 30-100 meshes.

[0019] The beneficial effects of the present invention are as follows: (1) the raw material apatite used in the present invention mainly provides calcium phosphate, the slag provides ferric oxide, and brings in titanium, manganese, vanadium, chromium, etc.; quartz, albite, quartz, and glass powder provide the necessary components for forming a vitreous body; the local inferior mud quartz with a high iron content is used to avoid the use of high-quality raw materials, and the high iron oxide content and the viscosity of the mud material are fully utilized, thereby rationally utilizing mineral resources and reducing material costs; the silicon, aluminum, calcium, iron, and phosphorus in the slag and apatite are used to replace part of the quartz, limestone, aluminum oxide, etc. in the dry granular materials, thereby saving mineral resources, reducing the use of reprocessed calcium phosphate and ferric oxide industrial products, and directly using minerals and slag to avoid waste in processing and production; the slag contains up to 50% iron oxide, and the use of slag avoids the instability and pollution caused by the direct use of ferric oxide;

[0020] (2) The present invention makes full use of low-cost materials such as apatite, slag, and glass powder, and according to the principle of crystallized glaze, adds a large amount of metal oxide iron oxide, dissolves ferric oxide in the phosphosilicate glass matrix to a saturated state, and when cooled, ferric oxide condenses and crystallizes due to supersaturation, becoming crystals suspended in the glaze; the glass body is quenched with water and broken into particles to form golden dry particles, which give people a golden and dazzling feeling; the golden dry particles can be used on the surface of ceramic tiles to form glittering particles similar to those in natural stones, and can also be used in full-polished glaze to form a starlight effect suspended in the glaze layer;

[0021] (3) The present invention uses slag as the main raw material, but the manganese dioxide contained in the slag will destroy the glass network structure composed of silicon dioxide and aluminum oxide, making the glass network structure loose. In step 1, a small amount of potassium dichromate combined with manganese dioxide is beneficial to Mn 3+ The direction of ion balance shifts in favor of Mn 3+ Generate and change the chemical structure of manganese dioxide, where Mn 3+ Oxidation-reduction reaction occurs with silicon ions in the glass matrix to form Mn 4+, thereby changing the atomic arrangement and bonding of the glass, and then changing the mechanical properties of the glass such as hardness, avoiding the destruction of the glass network structure, and the unreacted Mn 3+ It is purple, making the precipitated crystals golden purple. Under the irradiation of light, it not only has a metallic luster, but also presents a lavender glow, which is dazzling, novel and beautiful in color, elegant and noble, and improves the grade of the product. DETAILED DESCRIPTION

[0022] In order to better understand the present invention, the embodiments of the present invention are described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0023] In the following embodiments, the Jingyuan mud mine is 50 kilometers away from Yueyang County, in Sanjiang Town, Miluo City, and is a cohesive soil with a small sand content. Its appearance is light yellow, and after removing the surface red soil and vegetation, it contains less organic impurities and can be directly mined and used as a raw material for green bodies. When used as a raw material for glaze, it is first stirred into a mud with a specific gravity of 1.45g / cm3 in a slurry pool, passed through a 100-mesh vibrating screen, branches and large particles of sand and stone are removed, and squeezed into a mud cake and dried for standby use.

[0024] The chemical composition of the raw materials used in this example is shown in Table 1.

[0025] Table 1

[0026]

[0027] Embodiment 1:

[0028] A flash gold dry granule made from slag, the raw materials of which include, by weight, 25 parts of apatite, 30 parts of slag, 3 parts of zinc oxide, 12 parts of Jingyuan mud, 15 parts of albite, 15 parts of glass powder, and 10 parts of quartz. The chemical composition of the flash gold dry granule is, by mass percentage, SiO2 40%, Al2O3 9%, Fe2O3 13%, TiO2 0.6%, CaO 15%, MgO 0.5%, K2O 0.5%, Na2O 2.5%, ZnO 7%, MnO 1.2%, Cr2O3 0.4%, V2O5 0.3%, P2O5 10%.

[0029] After the above raw materials are processed and ground into 150-200 mesh powders, potassium dichromate solution is added to the slag for mixing and stirring, and then the raw material powders and the treated slag are weighed and mixed according to the above ratio, melted at 1260°C, cooled to 750°C and kept warm for 10 minutes, and quenched with water to obtain a metallic luster glass body, which is then crushed into particles with a particle size of 30-100 meshes to obtain flash gold dry particles; the potassium dichromate solution is obtained by weighing 0.5% of the weight of the slag and dissolving it in water.

[0030] Embodiment 2:

[0031] A flash gold dry granule made from slag, the raw materials of which include, by weight: 20 parts of apatite, 25 parts of slag, 5 parts of zinc oxide, 8 parts of Jingyuan mud, 10 parts of albite, 10 parts of glass powder, and 12 parts of quartz. The chemical composition of the flash gold dry granule is: by mass percentage, SiO2 34%, Al2O3 10%, Fe2O3 12%, TiO2 1.4%, CaO 20%, MgO 1.7%, K2O 0.8%, Na2O 1.5%, ZnO 6%, MnO 2 0.8%, Cr2O3 0.7%, V2O5 0.1%, P2O5 11%.

[0032] After the above raw materials are processed and ground into 150-200 mesh powders, potassium dichromate solution is added to the slag for mixing and stirring, and then the raw material powders and the treated slag are weighed and mixed according to the above ratio, melted at 1300°C, cooled to 650°C and kept warm for 10 minutes, and quenched with water to obtain a metallic luster glass body, which is then crushed into particles with a particle size of 30-100 meshes to obtain flash gold dry particles; the potassium dichromate solution is obtained by weighing 1% of the weight of the slag and dissolving it in water.

[0033] Embodiment 3:

[0034] A flash gold dry granule made from slag, the raw materials of which include, by weight, 30 parts of apatite, 20 parts of slag, 8 parts of zinc oxide, 15 parts of Jingyuan mud, 12 parts of albite, 13 parts of glass powder, and 5 parts of quartz. The chemical composition of the flash gold dry granule is, by mass percentage, SiO2 45%, Al2O3 8%, Fe2O3 11.7%, TiO2 0.5%, CaO 14%, MgO 1.6%, K2O 0.2%, Na2O 2.0%, ZnO 5%, MnO 1.0%, Cr2O3 0.3%, V2O5 0.2%, and P2O5 10.5%.

[0035] After the above raw materials are processed and ground into 150-200 mesh powders, potassium dichromate solution is added to the slag for mixing and stirring, and then the raw material powders and the treated slag are weighed and mixed according to the above ratio, melted at 1200°C, cooled to 730°C and kept warm for 10 minutes, and quenched with water to obtain a metallic luster glass body, which is then crushed into particles with a particle size of 30-100 meshes to obtain flash gold dry particles; the potassium dichromate solution is obtained by weighing 0.6% of the weight of the slag and dissolving it in water.

[0036] Comparative Example 1:

[0037] A flash gold dry granule made from slag, the raw materials of which include, by weight, 25 parts of apatite, 30 parts of slag, 3 parts of zinc oxide, 12 parts of Jingyuan mud, 15 parts of albite, 15 parts of glass powder, and 10 parts of quartz. The chemical composition of the flash gold dry granule is, by mass percentage, SiO2 40%, Al2O3 9%, Fe2O3 13%, TiO2 0.6%, CaO 15%, MgO 0.5%, K2O 0.5%, Na2O 2.5%, ZnO 7%, MnO 1.2%, Cr2O3 0.4%, V2O5 0.3%, P2O5 10%.

[0038] After the above raw materials are processed and ground into 150-200 mesh powders, the raw material powders are weighed and mixed according to the above ratios, melted at 1260°C, cooled to 750°C and kept warm for 10 minutes, and quenched with water to obtain a metallic luster glass body, which is then crushed into particles with a particle size of 30-100 mesh to obtain flash gold dry particles.

[0039] The physical properties of the dry gold particles obtained in Examples 1-3 and Comparative Example 1 were tested, and the test results are shown in Table 2.

[0040] Table 2

[0041]

[0042]

[0043] The above description of the embodiments is to facilitate the understanding and use of the present invention by those skilled in the art. Those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments. Improvements and modifications made by those skilled in the art based on the principles of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for producing flash gold dry particles made from slag, characterized in that: The production steps include: Step 1: crush the raw materials of apatite, slag, zinc oxide, Jingyuan mud, albite, glass powder and quartz into 150-200 mesh powder, add potassium dichromate solution to the slag, mix and stir, and treat them separately, then weigh and mix the raw material powders and the treated slag, melt them, and finally quench them with water to obtain a glass body with metallic luster crystals, wherein the raw material powders and the treated slag include, by weight: 20-30 parts of apatite, 20-30 parts of slag, 3-8 parts of zinc oxide, 8-15 parts of Jingyuan mud, 10-15 parts of albite, 10-15 parts of glass powder, and 5-12 parts of quartz; Step 2: crushing and sieving the glass obtained in step 1 to obtain flash gold dry particles; the chemical composition of the flash gold dry particles is: in mass percentage, SiO2 30-45%, Al2O3 5-10%, Fe2O3 10-13%, TiO2 0.5-1.4%, CaO 10-20%, MgO 0.5-1.7%, K2O 0.2-0.8%, Na2O 1.5-2.5%, ZnO 3-7%, MnO2 0.8-1.2%, Cr2O3 0.3-0.7%, V2O5 0.1-0.3%, P2O5 10-11%, and the sum of each chemical component is 100%.

2. The method for making flash gold dry particles made from slag according to claim 1, characterized in that: The raw material powders and the processed slag include, by weight: 25 parts of apatite, 30 parts of slag, 3 parts of zinc oxide, 12 parts of Jingyuan mud, 15 parts of albite, 15 parts of glass powder, and 10 parts of quartz.

3. The method for making flash gold dry particles made from slag according to claim 1, characterized in that: The potassium dichromate solution in step 1 is obtained by weighing 0.5-1% of potassium dichromate based on the weight of the slag and dissolving it in water.

4. The method for making flash gold dry particles made from slag according to claim 1, characterized in that: The melting temperature is 1200-1300°C.

5. The method for making flash gold dry particles made from slag according to claim 1, characterized in that: After the melting, the temperature is cooled to 650-750° C. and kept at this temperature for 10 minutes.

6. The method for making flash gold dry particles made from slag according to claim 1, characterized in that: The particle size of the flash gold dry particles is 30-100 meshes.

7. The method for making flash gold dry particles made from slag according to claim 1, characterized in that: The chemical composition of the flash gold dry particles is: in mass percentage, SiO2 40%, Al2O3 9%, Fe2O3 13%, TiO2 0.6%, CaO 15%, MgO 0.5%, K2O 0.5%, Na2O2 .5%, ZnO 7%, MnO2 1.2%, Cr2O3 0.4%, V2O5 0.3%, and P2O5 10%.