A preparation method of polyester composition and its application in rubber

By using polyester composition and functional additives in TBR tire tread rubber, combined with white carbon black and silane coupling agent, the shortcomings in the hardness and tear resistance of traditional rubber compositions are solved, and high stretching is achieved Comprehensive improvements in strength, low rolling resistance and good tear resistance.

CN116444953BActive Publication Date: 2024-11-15JIANGSU QIXIANG HIGH NEW MATERIAL
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202310367561.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-11-15
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

Traditional TBR tire tread rubber compositions are difficult to meet the requirements of high tensile strength, fixed stretch strength, wear resistance and low rolling resistance at the same time. Especially after using white carbon black instead of carbon black, the hardness and load-bearing capacity will be reduced and tear resistance will be resistant. There are also shortcomings in cracking and cutting resistance.

Method used

Using a polyester composition, including functional additives and polyester materials, the rubber composition is prepared by specific ratios and process steps (one stage kneading, two stage kneading, final kneading), using white carbon Black replaces carbon black, combined with silane coupling agent, optimizes the interface bonding of rubber, improves tear and cutting resistance, while maintaining or increasing hardness and tensile strength.

Benefits of technology

Compared with the NR/pure carbon black formula, the fixed stretch strength and hardness are comparable or higher, the tensile strength is consistent, the wear and tear resistance is better, the rolling resistance is significantly reduced, the tire bearing capacity is ensured, and the tire is significantly Improves the anti-vulcanization return performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The invention discloses a preparation method of a polyester composition and its application in rubber, and relates to the technical field of TBR tread rubber composition. The technical scheme is that the raw materials for preparing the rubber composition include the following components by weight: 100 parts of diene rubber, 0-70 parts of carbon black, 0-70 parts of white carbon black, 0-7 parts of silane coupling agent, 0.2-15 parts of polyester composition, 0.5-4 parts of vulcanizing agent and conventional auxiliary agents. The beneficial effect of the invention is that the invention provides a rubber composition that achieves the same or better tensile strength, tensile strength and hardness as the pure carbon black formula in the formula using white carbon black, ensures good load-bearing capacity of the tire, consistent wear resistance, and has more excellent tear resistance and cut resistance, significantly reduces rolling resistance, and has excellent anti-vulcanization reversion performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of TBR tread rubber compositions, and in particular to a preparation method of a polyester composition and application of the polyester composition in rubber. Background Art

[0002] Traditional TBR tire treads are mainly based on natural rubber, or some butadiene rubber is used in combination. The filler is mainly carbon black, which ensures good tensile strength, high elongation and hardness, high load-bearing capacity and good wear resistance. However, the rolling resistance of the carbon black rubber is very high, and it is difficult to ensure good tear resistance. The tread has poor resistance to collapse and sliding.

[0003] With the development of green tires, some white carbon black has been introduced to replace carbon black. It is used in combination with silane coupling agents to improve the interface bonding between fillers and rubber, reduce rolling resistance, and improve tear resistance. However, it leads to a decrease in hardness and tensile strength, a decrease in load-bearing capacity, and poor tread wear. It is difficult to ensure high tensile strength, high tensile strength, good wear resistance, reduce rolling resistance, and ensure good tear and cut resistance at the same time. Summary of the invention

[0004] In order to achieve the above-mentioned purpose of the invention and to solve the above-mentioned technical problems, the present invention provides a method for preparing a polyester composition and application thereof in rubber.

[0005] A polyester composition comprises at least one functional additive and at least one polyester material, wherein the functional additive has the following general structural formula:

[0006]

[0007] wherein R1-R4 are each independently hydrogen, a straight or branched alkyl group containing 3-24 carbon atoms, a cycloalkyl group containing 3-8 carbon atoms, an aralkyl group containing 7-26 carbon atoms, a phenyl group, or a phenyl group optionally substituted with a halogen atom, a nitro group and / or an OH group, or an alkylaryl group containing 7-26 carbon atoms, or form a heterocyclic ring containing 4-8 carbon atoms together with a specific nitrogen atom;

[0008] X is an integer from 2 to 6;

[0009] Y is or , wherein n is an integer of 0-6, and m is an integer of 1-3;

[0010] The polyester material is a reaction product of a polyol or anhydride and a polycarboxylic acid;

[0011] The mass ratio of the functional additive to the polyester material is 0.06-10.

[0012] The general structural formula 1 of the polyester material is as follows:

[0013]

[0014] wherein R1 is selected from a C2-C12 straight chain or branched saturated or unsaturated alkyl or alkyl-substituted aryl of a polycarboxylic acid or polyanhydride; R2 is selected from a C2-C12 straight chain or branched saturated or unsaturated alkyl; n is an integer between 2 and 200;

[0015] The general structural formula 2 of the polyester material is as follows:

[0016]

[0017] Wherein, R1 is selected from C2-C12 straight chain or branched saturated or unsaturated alkyl or alkyl substituted aryl; R2 is selected from C2-C12 straight chain or branched saturated or unsaturated alkyl; n is an integer between 2-200.

[0018] The polycarboxylic acid includes any one or more of oxalic acid (oxalic acid), succinic acid (succinic acid), trans-1,4-cyclohexanedicarboxylic acid, phthalic acid (anhydride), adipic acid, 3-carboxymethyl adipic acid, malonic acid, glutaric acid, maleic acid, 3-carboxy-4-hydroxyadipic acid, terephthalic acid, azelaic acid, toluene dicarboxylic acid, itaconic acid, pimelic acid, suberic acid, and sebacic acid.

[0019] The polyol includes any one or more of 1,4-butanediol, ethylene glycol, 1,3-propylene glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,10-decanediol, 1,12-dodecanediol, 1,20-eicosanediol, 1,4-cyclohexanedimethanol, isosorbide, o-phthalic alcohol, diethylene glycol, and cyclohexanediol.

[0020] The acid anhydride includes any one or more of oxalic anhydride, malonic anhydride, glutaric anhydride, succinic anhydride, adipic anhydride, hexahydrophthalic anhydride or 4-methylhexahydrophthalic anhydride, and maleic anhydride.

[0021] A rubber composition, comprising 100 parts of diene rubber, 0-70 parts of carbon black, 0-70 parts of white carbon black, 0-7 parts of silane coupling agent, 0.2-15 parts of polyester composition, 0.5-4 parts of vulcanizing agent and conventional additives;

[0022] Carbon black and white carbon black are not 0 at the same time;

[0023] The polyester composition is the polyester composition according to any one of claims 1 to 6.

[0024] The conventional auxiliary agents include 0.5-3 parts of stearic acid, 0.5-6 parts of zinc oxide, 0.5-5 parts of antioxidant, 0.5-4 parts of protective wax and 0.5-4 parts of accelerator.

[0025] The functional additive is 0.1-5 parts; the polyester material is 0.1-10 parts; and the white carbon black is 10-50 parts.

[0026] The diene rubber is selected from one of natural rubber and isoprene rubber or a combination thereof.

[0027] The method for preparing the rubber composition comprises the following steps:

[0028] (1) One-stage mixing: Diene rubber, white carbon black and carbon black are mixed in an internal mixer according to the mass ratio at a speed of 800 rpm. When the mixing temperature reaches 120°C, the mixer is cleaned and the speed is reduced to 50 rpm. The temperature is controlled at 140-150°C for rubber discharge. The mixer is opened to obtain a masterbatch.

[0029] (2) Second stage mixing: the rotation speed is 80 rpm, and the first stage masterbatch obtained in step (1) is added to the internal mixer according to the mass ratio, zinc oxide, stearic acid, antioxidant, antioxidant, the functional additive and the polyester material for mixing. When the mixing temperature reaches 120°C, the mixing is cleaned, the temperature is controlled at 140-150°C for glue discharge, and the second stage masterbatch is obtained by opening the mixer;

[0030] (3) Final rubber mixing: The second-stage masterbatch obtained in step (2), the vulcanizing agent and the accelerator are added to an internal mixer according to the mass ratio, the temperature is controlled at 95-100° C., and the rubber is discharged. The rubber is then rolled on an open mixer for 5 times and then cut into sheets to obtain the rubber composition.

[0031] The technical solution provided by the embodiment of the present invention has the following beneficial effects:

[0032] 1) The present invention overcomes the shortcomings of the prior art and provides a rubber composition that uses white carbon black instead of carbon black in a formula. Compared with the NR / pure carbon black formula, the present composition has equivalent or higher tensile strength and hardness, consistent tensile strength, higher elongation, equivalent wear, better tear and cut resistance, and significantly reduced rolling resistance, thereby ensuring good load-bearing capacity of the tire;

[0033] 2) The combination of functional additives and polyester has excellent anti-sulfurization reversion effect and a synergistic effect. DETAILED DESCRIPTION

[0034] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0035] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0036] The present invention is further described in detail in conjunction with the following specific examples. The sample preparation detection method and the like for implementing the invention, except for the contents specifically mentioned below, are all common knowledge and common common sense in the art, and the present invention has no special restrictions. The protection content of the present invention is not limited to the embodiments involved. Without departing from the spirit and scope of the inventive concept, the changes and advantages that can be thought of by those skilled in the art are included in the present invention, and the attached claims are the scope of protection.

[0037] Example 1

[0038] An embodiment of the present invention provides a polyester composition containing at least one functional auxiliary agent and at least one polyester material, including the following raw materials: 100 parts of natural rubber, 25 parts of carbon black N234, 25 parts of white carbon black HCSIL-833MP, 2 parts of Si69, 0.5 parts of the functional auxiliary agent A1 of the present invention, 1 part of the polyester material B1 of the present invention, 3.5 parts of zinc oxide, 1 part of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 1 part of protective wax, 1.1 parts of S, and 1.4 parts of accelerator NS.

[0039] The above raw materials by mass parts are mixed according to the following preparation method:

[0040] (1) One-stage mixing: Diene rubber, white carbon black and carbon black are mixed in an internal mixer according to the mass ratio at a speed of 800 rpm. When the mixing temperature reaches 120°C, the mixer is cleaned and the speed is reduced to 50 rpm. The temperature is controlled at 140-150°C for rubber discharge. The mixer is opened to obtain a masterbatch.

[0041] (2) Second stage mixing: the rotation speed is 80 rpm, and the first stage masterbatch obtained in step (1) is added to the internal mixer according to the mass ratio, zinc oxide, stearic acid, antioxidant, antioxidant, the functional additive and the polyester material for mixing. When the mixing temperature reaches 120°C, the mixing is cleaned, the temperature is controlled at 140-150°C for glue discharge, and the second stage masterbatch is obtained by opening the mixer;

[0042] (3) Final rubber mixing: The second-stage masterbatch obtained in step (2), the vulcanizing agent and the accelerator are added to an internal mixer according to the mass ratio, the temperature is controlled at 95-100° C., and the rubber is discharged. The rubber is then rolled on an open mixer for 5 times and then cut into sheets to obtain the rubber composition.

[0043] Example 2

[0044] An embodiment of the present invention provides a polyester composition containing at least one functional auxiliary agent and at least one polyester material, including the following raw materials: 100 parts of natural rubber, 50 parts of white carbon black HCSIL-833MP, 4 parts of Si69, 0.5 parts of the functional auxiliary agent A1 of the present invention, 1 part of the polyester material B1 of the present invention, 3.5 parts of zinc oxide, 1 part of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 1 part of protective wax, 1.1 parts of S, and 1.4 parts of accelerator NS.

[0045] The above raw materials in parts by mass were mixed according to the preparation method of Example 1 to prepare a rubber composition.

[0046] Example 3

[0047] An embodiment of the present invention provides a polyester composition containing at least one functional auxiliary agent and at least one polyester material, including the following raw materials: 100 parts of natural rubber, 50 parts of white carbon black HCSIL-833MP, 4 parts of Si69, 1 part of the functional auxiliary agent A1 of the present invention, 2 parts of the polyester material B1 of the present invention, 3.5 parts of zinc oxide, 1 part of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 1 part of protective wax, 1.1 parts of S, and 1.4 parts of accelerator NS.

[0048] The above raw materials in parts by mass were mixed according to the preparation method of Example 1 to prepare a rubber composition.

[0049] Example 4

[0050] An embodiment of the present invention provides a polyester composition containing at least one functional additive and at least one polyester material, including the following raw materials: 100 parts of natural rubber, 50 parts of white carbon black HCSIL-833MP, 4 parts of Si69, 0.5 parts of the functional additive A2 of the present invention, 1 part of the polyester material B2 of the present invention, 3.5 parts of zinc oxide, 1 part of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 1 part of protective wax, 1.1 parts of S, and 1.4 parts of accelerator NS.

[0051] The above raw materials in parts by mass were mixed according to the preparation method of Example 1 to prepare a rubber composition.

[0052] Example 5

[0053] An embodiment of the present invention provides a polyester composition containing at least one functional auxiliary agent and at least one polyester material, including the following raw materials: 100 parts of natural rubber, 50 parts of white carbon black HCSIL-833MP, 4 parts of Si69, 0.5 parts of the functional auxiliary agent A1 of the present invention, 1 part of the polyester material B2 of the present invention, 3.5 parts of zinc oxide, 1 part of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 1 part of protective wax, 1.1 parts of S, and 1.4 parts of accelerator NS.

[0054] The above raw materials in parts by mass were mixed according to the preparation method of Example 1 to prepare a rubber composition.

[0055] Example 6

[0056] An embodiment of the present invention provides a polyester composition containing at least one functional additive and at least one polyester material, including the following raw materials: 100 parts of natural rubber, 50 parts of white carbon black HCSIL-833MP, 4 parts of Si69, 0.5 parts of the functional additive A1 of the present invention, 1 part of the polyester material B3 of the present invention, 3.5 parts of zinc oxide, 1 part of stearic acid, 1 part of antioxidant 4020, 1 part of antioxidant RD, 1 part of protective wax, 1.1 parts of S, and 1.4 parts of accelerator NS.

[0057] The above raw materials in parts by mass were mixed according to the preparation method of Example 1 to prepare a rubber composition.

[0058] The functional additives and polyester structures selected in the comparative examples and example formulations are as follows:

[0059] Functional additive A1 structure:

[0060]

[0061] Functional additive A2 structure:

[0062]

[0063] Polyester material B1 structure:

[0064]

[0065] Polyester material B2 structure:

[0066]

[0067] Polyester material B3 structure:

[0068]

[0069] The formula comparison of Comparative Examples 1-5 and Examples 1-7 is shown in Table 1:

[0070] Table 1

[0071]

[0072] Rubber composition performance test specifications:

[0073] The rubber compounds prepared from the reference formulation and the example formulation were tested according to the following standards:

[0074] Vulcanization performance test: Refer to GB / T 16584-1996 to test the vulcanization performance of the rubber compound;

[0075] Mechanical properties test: Tested according to GB / T528-2009;

[0076] Vulcanized rubber hardness: hardness test according to GBT531.1-2008;

[0077] The hot air aging test is carried out according to GB / T 3512-2014 "Hot air accelerated aging and heat resistance test for vulcanized rubber or thermoplastic rubber". The test conditions are: 100℃×72h. Each sample is tested with 5 samples, and the test result is the median value.

[0078] DIN abrasion: abrasion test is carried out according to GBT 9867-2008 "Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrasion machine method)";

[0079] DMA test: Dynamic mechanical analysis is used to test the vulcanized rubber. The test conditions are: the test mode is tensile mode, the dynamic strain is 0.25%, the static strain is 1%, and the heating rate is 3K / min. The smaller the tanδ value at 60℃, the lower the heat generation value of the tread rubber;

[0080] Cutting resistance test: Cutting loss test principle: Use a specially designed cutter head to repeatedly impact a rotating round rubber sample with a certain amount of energy. Simulate the tire hitting a sharp object with considerable force, the surface is cut, and simulate the tire tread on a rough and sharp road surface, cutting, tearing, and chipping caused by traction or braking. The cutting loss is expressed by the weight difference of the rubber sample before and after the test, and is implemented according to the enterprise standard. The speed is 720r / min, the impact frequency is 120 / min, and the test time is 10min. The lower the cutting loss value, the better the cutting resistance performance.

[0081] Sources of other components in the embodiments and comparative examples:

[0082] Natural rubber, SCR5, Yunken Jiangcheng Rubber Company

[0083] Carbon black, N234, Shanghai Cabot Chemical Co., Ltd.

[0084] White carbon black, HCSIL-833MP, Wuxi Hengcheng Silicon Industry Co., Ltd.

[0085] Zinc Oxide, Shiyang Zinc Technology (Huai'an) Co., Ltd.

[0086] Stearic acid, Nantong Yuhao Chemical Technology Co., Ltd.

[0087] Antiaging agent RD, Henan Kailun Chemical Co., Ltd.

[0088] Antioxidant 4020, Henan Kailun Chemical Co., Ltd.

[0089] Sulfur powder, Linyi Guoao Co., Ltd.

[0090] Accelerator NS, Kemai Chemical Co., Ltd.

[0091] The instruments and equipment used in the comparative examples and embodiments are:

[0092] Mixing mill, a product of Farrell Corporation of the United States

[0093] BR1600 internal mixer, a product of Farrell, USA

[0094] VR-7130 Dynamic Mechanical Analyzer, Ueshima Manufacturing Co., Ltd.

[0095] P-80-pcd-3L Plate Vulcanizing Machine, Pan Petroleum Industry

[0096] M-3000A rotorless rheometer, High Speed ​​Rail Testing Instrument Co., Ltd.

[0097] MV-3000 Mooney Viscometer, High Speed ​​Rail Testing Instrument Co., Ltd.

[0098] AL-7000S tensile machine, High Speed ​​Rail Testing Instrument Co., Ltd.

[0099] GT-7016-AR cutting machine, High Speed ​​Rail Testing Instrument Co., Ltd.

[0100] LX-A Hardness Tester, Jiangsu Mingzhu Testing Machinery Co., Ltd.

[0101] RCC-I Rubber Dynamic Cutting Tester, Beijing Wanhui Yifang Technology Development Co., Ltd.

[0102] The performance test comparison of Comparative Examples 1-5 and Examples 1-7 is shown in Table 2:

[0103] Table 2

[0104]

[0105] R95 can be used to characterize the anti-vulcanization reversion effect of the rubber compound. The larger the R95 value, the better the anti-vulcanization reversion effect of the rubber compound, and there is a strong correlation. The DMA test can use 60℃ tanδ to characterize the rolling resistance of the tread rubber compound. The lower the value, the lower the rolling resistance of the tread rubber compound.

[0106] From the above data, it can be seen that when the composition of the present invention is used, after 25 parts of white carbon black replaces carbon black, the hardness and tensile strength decrease, and the wear becomes worse. When functional additives A1 and polyester material B1 are used alone, some performance is improved, but both have performance disadvantages. When the two are used in combination, compared with the carbon black system, the hardness and tensile strength are at a higher level, the tensile strength and abrasion remain at the same level, the elongation at break is significantly improved, the cutting resistance reduction is significantly reduced, the DMA data 60℃ tanδ is significantly reduced, the rolling resistance is significantly reduced, and the physical properties after aging remain at a higher level, and the anti-sulfurization reversion performance is also significantly improved. The pure white carbon black formula is used in combination with functional additives A1 and polyester material B1, and the overall performance improvement is more obvious. Functional additives A2, functional additives A3 and polyester materials B2, polyester materials B3 also show good comprehensive performance. The composition of the present invention has important reference value for comprehensively improving the performance of TBR tire tread rubber and improving tire durability.

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A polyester composition, It is characterized in that It includes at least one functional auxiliary agent and at least one polyester material, and the general structural formula of the functional auxiliary agent is as follows: Among them, R 1 -R 4 are each independently hydrogen, a straight or branched alkyl group containing 3 to 24 carbon atoms, a cycloalkyl group containing 3 to 8 carbon atoms, an aralkyl group containing 7 to 26 carbon atoms, a phenyl group, or a phenyl group optionally substituted with a halogen atom, a nitro group and / or an OH group, or an alkylaryl group containing 7 to 26 carbon atoms, or form a heterocyclic ring containing 4 to 8 carbon atoms with a specific nitrogen atom; X is an integer from 2 to 6; Y is , where n is an integer from 0 to 6; The polyester material is a reaction product of a polyol and anhydride or polycarboxylic acid; The mass ratio of the functional additive to the polyester material is 0.06-10; The general structural formula 1 of the polyester material is as follows: Among them, R 1 A C2-C12 straight or branched saturated or unsaturated alkyl or alkyl-substituted aryl group selected from polycarboxylic acids or polyanhydrides; R 2 Selected from C2-C12 straight chain or branched saturated or unsaturated alkyl; n is an integer between 2 and 200; The general structural formula 2 of the polyester material is as follows: Among them, R 1 is selected from C2-C12 straight chain or branched saturated or unsaturated alkyl or alkyl substituted aryl; 2 is selected from C2-C12 straight chain or branched saturated or unsaturated alkyl; n is an integer between 2-200.

2. A polyester composition according to claim 1, It is characterized in that The polycarboxylic acid includes any one or more of succinic acid, adipic acid, glutaric acid, maleic acid, azelaic acid, toluene dicarboxylic acid, itaconic acid, pimelic acid, suberic acid, and sebacic acid.

3. A polyester composition according to claim 1, It is characterized in that The polyol includes any one or more of 1,4-butanediol, ethylene glycol, 1,3-propylene glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,10-decanediol, and 1,12-dodecanediol.

4. A polyester composition according to claim 1, It is characterized in that The acid anhydride includes any one or more of glutaric anhydride, succinic anhydride, adipic anhydride and maleic anhydride.

5. A rubber composition, It is characterized in that The rubber composition comprises 100 parts of diene rubber, 0-70 parts of carbon black, 0-70 parts of white carbon black, 0-7 parts of silane coupling agent, 0.2-15 parts of polyester composition, 0.5-4 parts of vulcanizing agent and conventional additives; The conventional additives include 0.5-3 parts of stearic acid, 0.5-6 parts of zinc oxide, 0.5-5 parts of antioxidant, 0.5-4 parts of protective wax, and 0.5-4 parts of accelerator; carbon black and white carbon black are not 0 at the same time; The polyester composition is the polyester composition according to any one of claims 1 to 4.

6. A rubber composition according to claim 5, It is characterized in that The functional additive is 0.1-5 parts; the polyester material is 0.1-10 parts; and the white carbon black is 10-50 parts.

7. A rubber composition according to claim 5, It is characterized in that The diene rubber is selected from natural rubber and isoprene rubber or a combination thereof.

8. A rubber composition according to claim 5, It is characterized in that The method for preparing the rubber composition comprises the following steps: (1) One-stage mixing: Diene rubber, white carbon black and carbon black are mixed in an internal mixer according to the mass ratio at a speed of 800 rpm. When the mixing temperature reaches 120°C, the mixer is cleaned and the speed is reduced to 50 rpm. The temperature is controlled at 140-150°C for rubber discharge. The mixer is opened to obtain a masterbatch. (2) Second stage mixing: the rotation speed is 80 rpm, and the first stage masterbatch obtained in step (1) is added to the internal mixer according to the mass ratio, zinc oxide, stearic acid, antioxidant, the functional additive and the polyester material for mixing. When the mixing temperature reaches 120°C, the mixing is cleaned, the temperature is controlled at 140-150°C for glue discharge, and the second stage masterbatch is obtained by opening the mixer; (3) Final rubber mixing: The second-stage masterbatch obtained in step (2), the vulcanizing agent and the accelerator are added to an internal mixer according to the mass ratio, the temperature is controlled at 95-100° C., and the rubber is discharged. The rubber is then rolled on an open mixer for 5 times and then cut into sheets to obtain the rubber composition.

Citation Information

Patent Citations

  • Formula of highly anti-fatigue automobile brake chamber rubber diaphragm material

    CN101302311A

  • Sulfide modified elastomeric polymers

    CN101610917A

  • Rubber composition for tire and studless tire

    CN106459507A

  • Polyester resin composite material for instruments and apparatus

    CN107118519A

  • High-strength plastic for building industry

    CN107418129A