A functionalized low-temperature heat-sealing material and its application
By grafting polyamide into polypropylene chains, the heat-sealing material achieves strong adhesion to metals and papers, addressing the sealing challenges of polypropylene films with enhanced tensile and heat-seal strengths.
Patent Information
- Application Number
- CN202310541086.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-15
AI Technical Summary
Polypropylene films face challenges in heat sealing due to high crystallinity and poor adhesion to metals and papers, despite modifications like copolymerization with polyamides, which do not yield satisfactory results.
A functionalized low-temperature heat-sealing material is developed by grafting polyamide with a specific structure into the polypropylene molecular chain, combined with metallocene polyethylene and propylene-based elastomer, to enhance adhesion and reduce crystallinity.
The solution results in a low-temperature heat-sealing film with strong adhesion to metals and papers, high tensile strength, low heat shrinkage, and improved heat-seal strength, as demonstrated by performance tests on aluminum-plastic composite films.
Smart Images

Figure BDA0004227952380000021 
Figure BDA0004227952380000041 
Figure BDA0004227952380000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat-sealing films, and in particular relates to a functionalized low-temperature heat-sealing material and an application thereof. Background Art
[0002] Polypropylene is one of the five general-purpose plastics and a widely used thermoplastic molding material with excellent rigidity, heat resistance and transparency. It is often used as a flexible packaging material for food, clothing, medicines and other items. In daily use, in order to form packaging materials, it is necessary to seal between different sheets or different parts made of film materials, usually by heat sealing the materials. Polypropylene is a crystalline polymer. A single-layer film composed of crystalline polypropylene will shrink at the heat sealing temperature, making it difficult to heat seal such films. Therefore, in order to reduce the crystallinity of polypropylene, comonomers such as ethylene, butene, hexene, etc. are commonly used in industry to copolymerize or blend polypropylene.
[0003] The crystallinity of polypropylene is reduced to a certain extent by copolymerization modification or blending modification, but the polarity of polyolefin is weak, and the modified heat-sealing film still has the problem of poor adhesion to metal or paper. The existing technology copolymerizes or blends polypropylene copolymers through polyamide to improve the adhesion between the heat-sealing film and metal or paper, but the effect is not ideal. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a functionalized low-temperature heat-sealing material, by grafting polyamide with a specific structure into the polypropylene molecular chain to obtain a low-temperature heat-sealing film with strong adhesion to metal or paper.
[0005] In a first aspect of the present invention, a functionalized low-temperature heat-sealing material is provided, comprising the following raw materials in parts by weight: 20 to 30 parts of polypropylene grafted polyamide, 10 to 15 parts of metallocene polyethylene, and 5 to 10 parts of propylene-based elastomer;
[0006] The polypropylene grafted polyamide is prepared by reacting amino grafted PP, ester monomers and ethylenediamine in a weight ratio of 0.05-0.2:1:2-10;
[0007] The ester monomer structure is as follows:
[0008]
[0009] Preferably, the preparation of the polypropylene grafted polyamide comprises the following steps:
[0010] Ester monomers and ethylenediamine are mixed according to weight ratio, methanol is added for reaction, amino-grafted PP, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, N-hydroxysuccinimide and water are added, pH value is adjusted, and stirring is performed to obtain polypropylene grafted polyamide.
[0011] Preferably, the weight ratio of the ester monomer to 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 1:1:0.5-1.5.
[0012] Preferably, the pH value is adjusted to less than 6.
[0013] Preferably, the reaction temperature is 50-60°C.
[0014] More preferably, the reaction temperature is 55°C.
[0015] Preferably, the reaction time is 12 to 18 hours.
[0016] More preferably, the reaction time is 15 hours.
[0017] Preferably, the stirring time is 2 to 3 hours.
[0018] More preferably, the stirring time is 2.5 hours.
[0019] Preferably, the metallocene polyethylene has a melt index of 3 to 5 g / 10 min at 190°C.
[0020] Preferably, the melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is greater than 10 g / 10 min.
[0021] In a second aspect, the present invention provides a low-temperature heat-sealing film, comprising an inner layer and an outer layer, wherein the inner layer is a heat-sealing layer, and the heat-sealing layer is made of the functionalized low-temperature heat-sealing material.
[0022] Preferably, the thickness of the inner layer is 1 to 36 μm.
[0023] More preferably, the thickness of the inner layer is 2 μm
[0024] Preferably, the outer layer is composed of atactic polypropylene and isotactic polypropylene in a weight ratio of 1:3-5.
[0025] More preferably, the outer layer consists of atactic polypropylene and isotactic polypropylene in a weight ratio of 1:4.
[0026] Preferably, the thickness of the outer layer is 8-15 μm.
[0027] More preferably, the thickness of the outer layer is 10 μm.
[0028] In a third aspect of the present invention, a method for preparing the low-temperature heat-sealing film is provided, comprising the following steps:
[0029] S1. The raw materials for the inner layer and the outer layer are added through the feeding port of the extruder, heated and extruded, melted and plasticized, and their respective melts are obtained;
[0030] S2. Cast the melt from the die of the extruder, stretch it biaxially, cool it to form a film, perform corona treatment, and wind it up to obtain a low-temperature heat-sealed film.
[0031] Preferably, the inner layer is heated and extruded at temperatures of 175° C., 190° C., and 210° C. in sequence.
[0032] Preferably, the outer layer is heated and extruded at temperatures of 185°C, 205°C and 215°C in sequence.
[0033] Preferably, the cooling temperature is 28-32°C. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0035] Amino-grafted PP is amino-grafted polypropylene, which is commercially available.
[0036] Example 1: Preparation of polypropylene grafted polyamide.
[0037] Under nitrogen protection, 10 parts by weight of ester monomer and 20 parts by weight of ethylenediamine were added to a reaction bottle and mixed, 20 parts by weight of methanol were added, and the mixture was reacted at 55° C. for 15 hours, 2 parts by weight of amino-grafted PP, 10 parts by weight of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, 15 parts by weight of N-hydroxysuccinimide and 50 parts by weight of water were added, the pH value was adjusted to 2.5-3.5, and the mixture was stirred for 2.5 hours to obtain polypropylene grafted polyamide;
[0038] The structure of the ester monomer is as follows:
[0039]
[0040] Example 2: Preparation of polypropylene grafted polyamide.
[0041] Under nitrogen protection, 10 parts by weight of ester monomer and 100 parts by weight of ethylenediamine were added to a reaction bottle and mixed, 20 parts by weight of methanol were added, and the mixture was reacted at 55° C. for 15 hours, 0.5 parts by weight of amino-grafted PP, 10 parts by weight of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, 5 parts by weight of N-hydroxysuccinimide and 50 parts by weight of water were added, the pH value was adjusted to 2.5-3.5, and the mixture was stirred for 2.5 hours to obtain polypropylene grafted polyamide;
[0042] The structure of the ester monomer is as follows:
[0043]
[0044] Example 3: Preparation of polypropylene grafted polyamide.
[0045] Under nitrogen protection, 10 parts by weight of ester monomer and 50 parts by weight of ethylenediamine were added to a reaction bottle and mixed, 20 parts by weight of methanol were added, and the mixture was reacted at 55° C. for 15 hours, 1 part by weight of amino-grafted PP, 10 parts by weight of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, 10 parts by weight of N-hydroxysuccinimide and 50 parts by weight of water were added, the pH value was adjusted to 2.5-3.5, and the mixture was stirred for 2.5 hours to obtain polypropylene grafted polyamide;
[0046] The structure of the ester monomer is as follows:
[0047]
[0048] Example 4: Preparation of low temperature heat-sealing film.
[0049] S1. 20 parts by weight of the polypropylene grafted polyamide obtained in Example 1, 15 parts by weight of metallocene polyethylene, and 10 parts by weight of a propylene-based elastomer were added to the extruder through the feed port of the extruder, and heated and extruded at 175°C, 190°C, and 210°C, respectively, and melt-plasticized to obtain an inner layer melt;
[0050] S2. 10 parts by weight of random polypropylene and 40 parts by weight of isotactic polypropylene were added through the feed port of the extruder, and heated and extruded at temperatures of 185°C, 205°C, and 215°C, melt-plasticized to obtain an outer molten body;
[0051] S3. The inner layer melt and the outer layer melt are cast from the die of the extruder, biaxially stretched, the longitudinal stretching unit temperature is controlled at 60-150°C, the transverse stretching unit temperature is controlled at 100-180°C, the longitudinal stretching ratio is controlled at 4-6, the transverse stretching ratio is controlled at 6-10, cooled at 28-32°C to form a film, corona, and rolled to obtain a low-temperature heat-seal film of 12 μm with an inner layer thickness of 2 μm and an outer layer thickness of 10 μm;
[0052] The metallocene polyethylene has a melt index of 3 g / 10 min at 190° C.;
[0053] The melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is 12 g / 10 min.
[0054] Example 5: Preparation of low temperature heat-sealing film.
[0055] S1. 30 parts by weight of the polypropylene grafted polyamide obtained in Example 2, 10 parts by weight of metallocene polyethylene, and 5 parts by weight of a propylene-based elastomer were added to the extruder through the feed port of the extruder, and heated and extruded at temperatures of 175°C, 190°C, and 210°C, respectively, and melt-plasticized to obtain an inner layer melt;
[0056] S2. 10 parts by weight of random polypropylene and 40 parts by weight of isotactic polypropylene were added through the feed port of the extruder, and heated and extruded at temperatures of 185°C, 205°C, and 215°C, melt-plasticized to obtain an outer molten body;
[0057] S3. The inner layer melt and the outer layer melt are cast from the die of the extruder, biaxially stretched, the longitudinal stretching unit temperature is controlled at 60-150°C, the transverse stretching unit temperature is controlled at 100-180°C, the longitudinal stretching ratio is controlled at 4-6, the transverse stretching ratio is controlled at 6-10, cooled at 28-32°C to form a film, corona, and rolled to obtain a low-temperature heat-seal film of 12 μm with an inner layer thickness of 2 μm and an outer layer thickness of 10 μm;
[0058] The metallocene polyethylene has a melt index of 4 g / 10 min at 190° C.;
[0059] The melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is 15 g / 10 min.
[0060] Example 6: Preparation of low temperature heat-sealing film.
[0061] S1. 25 parts by weight of the polypropylene grafted polyamide obtained in Example 3, 12 parts by weight of metallocene polyethylene, and 8 parts by weight of a propylene-based elastomer were added to the extruder through the feed port of the extruder, and heated and extruded at temperatures of 175°C, 190°C, and 210°C, respectively, and melt-plasticized to obtain an inner layer melt;
[0062] S2. 10 parts by weight of random polypropylene and 40 parts by weight of isotactic polypropylene were added through the feed port of the extruder, and heated and extruded at temperatures of 185°C, 205°C, and 215°C, melt-plasticized to obtain an outer molten body;
[0063] S3. The inner layer melt and the outer layer melt are cast from the die of the extruder, biaxially stretched, the longitudinal stretching unit temperature is controlled at 60-150°C, the transverse stretching unit temperature is controlled at 100-180°C, the longitudinal stretching ratio is controlled at 4-6, the transverse stretching ratio is controlled at 6-10, cooled at 28-32°C to form a film, corona, and rolled to obtain a low-temperature heat-seal film of 12 μm with an inner layer thickness of 2 μm and an outer layer thickness of 10 μm;
[0064] The metallocene polyethylene has a melt index of 5 g / 10 min at 190° C.;
[0065] The melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is 18 g / 10 min.
[0066] Comparative Example 1: Preparation of low-temperature heat-sealing film.
[0067] S1. Under nitrogen protection, 10 parts by weight of methyl acrylate and 50 parts by weight of ethylenediamine were added to a reaction flask and mixed, 20 parts by weight of methanol were added, and the mixture was reacted at 55°C for 15 hours, 1 part by weight of amino-grafted PP, 10 parts by weight of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, 10 parts by weight of N-hydroxysuccinimide and 50 parts by weight of water were added, the pH value was adjusted to 2.5 to 3.5, and stirred for 2.5 hours to obtain polypropylene grafted polyamide;
[0068] S2. 25 parts by weight of the polypropylene grafted polyamide obtained in S1, 12 parts by weight of metallocene polyethylene, and 8 parts by weight of a propylene-based elastomer were added to the extruder through the feed port of the extruder, and heated and extruded at temperatures of 175°C, 190°C, and 210°C, melt-plasticized, and the inner layer melt was obtained;
[0069] S3. 10 parts by weight of random polypropylene and 40 parts by weight of isotactic polypropylene were added through the feed port of the extruder, and heated and extruded at temperatures of 185°C, 205°C, and 215°C, melt-plasticized to obtain an outer layer of melt;
[0070] S4. The inner layer melt and the outer layer melt are cast from the die of the extruder, biaxially stretched, the longitudinal stretching unit temperature is controlled at 60-150°C, the transverse stretching unit temperature is controlled at 100-180°C, the longitudinal stretching ratio is controlled at 4-6, the transverse stretching ratio is controlled at 6-10, cooled at 28-32°C to form a film, corona, and rolled to obtain a low-temperature heat-seal film of 12 μm with an inner layer thickness of 2 μm and an outer layer thickness of 10 μm;
[0071] The metallocene polyethylene has a melt index of 5 g / 10 min at 190° C.;
[0072] The melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is 18 g / 10 min.
[0073] Comparative Example 2: Preparation of low-temperature heat-sealing film.
[0074] S1. 25 parts by weight of the polypropylene grafted polyamide obtained in Example 3, 12 parts by weight of metallocene polyethylene, and 8 parts by weight of a propylene-based elastomer were added to the extruder through the feed port of the extruder, and heated and extruded at temperatures of 175°C, 190°C, and 210°C, respectively, and melt-plasticized to obtain an inner layer melt;
[0075] S2. 10 parts by weight of random polypropylene and 40 parts by weight of isotactic polypropylene were added through the feed port of the extruder, and heated and extruded at temperatures of 185°C, 205°C, and 215°C, melt-plasticized to obtain an outer molten body;
[0076] S3. The inner layer melt and the outer layer melt are cast from the die of the extruder, biaxially stretched, the longitudinal stretching unit temperature is controlled at 60-150°C, the transverse stretching unit temperature is controlled at 100-180°C, the longitudinal stretching ratio is controlled at 4-6, the transverse stretching ratio is controlled at 6-10, cooled at 28-32°C to form a film, corona, and rolled to obtain a low-temperature heat-seal film of 12 μm with an inner layer thickness of 2 μm and an outer layer thickness of 10 μm;
[0077] The metallocene polyethylene has a melt index of 1 g / 10 min at 190° C.;
[0078] The melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is 18 g / 10 min.
[0079] Comparative Example 3: Preparation of low-temperature heat-sealing film.
[0080] S1. 25 parts by weight of the polypropylene grafted polyamide obtained in Example 3, 12 parts by weight of metallocene polyethylene, and 8 parts by weight of a propylene-based elastomer were added to the extruder through the feed port of the extruder, and heated and extruded at temperatures of 175°C, 190°C, and 210°C, respectively, and melt-plasticized to obtain an inner layer melt;
[0081] S2. 10 parts by weight of random polypropylene and 40 parts by weight of isotactic polypropylene were added through the feed port of the extruder, and heated and extruded at temperatures of 185°C, 205°C, and 215°C, melt-plasticized to obtain an outer molten body;
[0082] S3. The inner layer melt and the outer layer melt are cast from the die of the extruder, biaxially stretched, the longitudinal stretching unit temperature is controlled at 60-150°C, the transverse stretching unit temperature is controlled at 100-180°C, the longitudinal stretching ratio is controlled at 4-6, the transverse stretching ratio is controlled at 6-10, cooled at 28-32°C to form a film, corona, and rolled to obtain a low-temperature heat-seal film of 12 μm with an inner layer thickness of 2 μm and an outer layer thickness of 10 μm;
[0083] The metallocene polyethylene has a melt index of 7 g / 10 min at 190° C.;
[0084] The melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is 18 g / 10 min.
[0085] Comparative Example 4: Preparation of low-temperature heat-sealing film.
[0086] S1. 25 parts by weight of the polypropylene grafted polyamide obtained in Example 3, 12 parts by weight of metallocene polyethylene, and 8 parts by weight of a propylene-based elastomer were added to the extruder through the feed port of the extruder, and heated and extruded at temperatures of 175°C, 190°C, and 210°C, respectively, and melt-plasticized to obtain an inner layer melt;
[0087] S2. 10 parts by weight of random polypropylene and 40 parts by weight of isotactic polypropylene were added through the feed port of the extruder, and heated and extruded at temperatures of 185°C, 205°C, and 215°C, melt-plasticized to obtain an outer molten body;
[0088] S3. The inner layer melt and the outer layer melt are cast from the die of the extruder, biaxially stretched, the longitudinal stretching unit temperature is controlled at 60-150°C, the transverse stretching unit temperature is controlled at 100-180°C, the longitudinal stretching ratio is controlled at 4-6, the transverse stretching ratio is controlled at 6-10, cooled at 28-32°C to form a film, corona, and rolled to obtain a low-temperature heat-seal film of 12 μm with an inner layer thickness of 2 μm and an outer layer thickness of 10 μm;
[0089] The metallocene polyethylene has a melt index of 5 g / 10 min at 190° C.;
[0090] The melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is 5 g / 10 min.
[0091] Performance test: The inner layer of the low-temperature heat-sealing film of Examples 4 to 6 and Comparative Examples 1 to 4 was compounded with an aluminum foil having a thickness of 50 μm to obtain aluminum-plastic composite films of Examples 7 to 9 and Comparative Examples 5 to 8, respectively. The performance tests were carried out with reference to GB / T12026-2000. The test results are shown in Table 1.
[0092] Table 1. Test results of properties of aluminum-plastic composite films.
[0093]
[0094]
[0095] As can be seen from Table 1, the aluminum-plastic composite films of Examples 7-9 prepared from the low-temperature heat-seal films of Examples 4-6 have strong adhesion, high tensile strength, low heat shrinkage, high heat-seal strength and low haze; the low-temperature heat-seal film of Comparative Example 5 uses polyamide-modified polypropylene prepared from conventional methyl acrylate monomer, and the prepared aluminum-plastic composite film has high heat-seal temperature, high heat shrinkage, low heat-seal strength, high haze and low peel strength; the metallocene polyethylene of Comparative Example 6 has a melt index of less than 3g / 10min at 190°C, and the prepared aluminum-plastic composite film has a high heat-seal temperature and low tensile strength; the metallocene polyethylene of Comparative Example 7 has a melt index of more than 5g / 10min at 190°C, and the prepared aluminum-plastic composite film has low peel strength, high heat shrinkage, high heat-seal temperature and low heat-seal strength; the propylene-based elastomer of Comparative Example 8 has a melt flow rate of less than 10g / 10min at 230°C and under a load of 2.16kg, and the prepared aluminum-plastic composite film has high haze.
[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that after reading the specification of this application, the technicians can still modify or replace the specific implementation mode of the present invention with equivalents, but these modifications or changes do not deviate from the scope of protection of the pending claims of the present application.
Claims
1. A functionalized low-temperature heat-sealing material, It is characterized in that The invention comprises the following raw materials in parts by weight: 20 to 30 parts of polypropylene grafted polyamide, 10 to 15 parts of metallocene polyethylene, and 5 to 10 parts of propylene-based elastomer; the melt index of the metallocene polyethylene at 190° C. is 3 to 5 g / 10 min; the melt flow rate of the propylene-based elastomer at 230° C. and under a load of 2.16 kg is greater than 10 g / 10 min; The polypropylene grafted polyamide is prepared by reacting amino grafted PP, ester monomers and ethylenediamine in a weight ratio of 0.05-0.2:1:2-10; The ester monomer structure is as follows: The preparation of the polypropylene grafted polyamide comprises the following steps: Ester monomers and ethylenediamine are mixed according to weight ratio, methanol is added to react at 50-60°C for 12-18 hours, amino-grafted PP, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, N-hydroxysuccinimide and water are added, the pH value is adjusted to less than 6, and stirred for 2-3 hours to obtain polypropylene grafted polyamide.
2. The functionalized low-temperature heat-sealing material according to claim 1, It is characterized in that The weight ratio of the ester monomer to 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 1:1:0.5-1.
5.
3. A low temperature heat-sealing film, It is characterized in that It comprises an inner layer and an outer layer, wherein the inner layer is a heat-sealing layer, and the heat-sealing layer is made of the functionalized low-temperature heat-sealing material according to any one of claims 1 to 2.
4. The low-temperature heat-sealing film according to claim 3, It is characterized in that The thickness of the inner layer is 1 to 36 μm.
5. The low-temperature heat-sealing film according to claim 3, It is characterized in that The outer layer is composed of atactic polypropylene and isotactic polypropylene in a weight ratio of 1:3-5.
6. The low-temperature heat-sealing film according to claim 3, It is characterized in that The thickness of the outer layer is 8-15 μm.