A two-component fire-resistant flame-retardant heat-insulating coating and its application in automobile production
By adding fire-resistant, flame-retardant and heat-insulating agents such as aluminum hydroxide, antimony trioxide, perlite and modified kaolin to automotive coatings, the problem of the lack of fire-retardant, flame-retardant and heat-insulating properties of existing coatings is solved, and the performance of the coatings is significantly improved. Fire-resistant, flame-retardant and heat-insulating effects meet the needs of automotive coatings in fire protection and thermal management.
Patent Information
- Application Number
- CN202310447560.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-04-24
AI Technical Summary
Existing water-based two-component acrylic polyurethane automotive coatings lack fire-retardant and heat-insulating properties, making it difficult to meet the needs of automotive coatings in terms of fire protection and thermal management.
A fire-resistant, flame-retardant and heat-insulating agent composed of aluminum hydroxide, antimony trioxide, perlite and modified kaolin is added to the two-component paint, and the performance of the kaolin is improved through modification treatment to enhance the fire-retardant, flame-retardant and heat insulation of the paint. Effect.
The fire-retardant, flame-retardant and heat-insulating properties of the two-component fire-resistant, flame-retardant and heat-insulating coating are significantly improved, the fire-resistant limit time is extended, the thermal conductivity is reduced, and the fire protection and thermal management capabilities of the coating are significantly improved.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating preparation, and in particular to a two-component fire-resistant, flame-retardant and heat-insulating coating and application thereof in automobile production. Background Art
[0002] Automotive coatings refer to coatings applied to the bodies and parts of various types of vehicles such as cars; they include coatings for new cars and coatings for vehicle repairs.
[0003] Chinese invention patent 201010548579.7 provides a water-based two-component acrylic polyurethane automotive coating and its preparation method; it is prepared from component A and component B, wherein component A is prepared by adding a formula amount of water-based hydroxyl resin, a wetting agent, a defoamer, a thickener, a coupling agent, and a film-forming aid into deionized water and dispersing for 15 minutes; component B is a polyisocyanate curing agent, component B is weighed according to the formula amount, and component B is slowly added to component A in a dispersed state, and continued to disperse for 5 minutes to obtain the coating. The water-based two-component automotive coating prepared by the invention retains the original hardness, medium resistance and salt spray resistance of the coating film, and the VOC content is greatly reduced. It is widely used in the water-based automotive coating industry and has great industrial application value and market prospects.
[0004] However, the inventors found in actual applications that the above-mentioned water-based two-component acrylic polyurethane automotive coating does not have fire retardant and heat insulation properties, and needs further improvement. Summary of the invention
[0005] In order to overcome at least one of the technical problems existing in the prior art, the present invention provides a two-component fire-resistant, flame-retardant and heat-insulating coating and a preparation method thereof.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] A two-component fire-resistant flame-retardant heat-insulating coating, comprising component A and component B; the component A comprises a water-based hydroxyl resin, an additive and water; the component B is a curing agent; the component A also comprises a fire-resistant flame-retardant heat-insulating agent;
[0008] The fire-resistant flame-retardant heat-insulating agent comprises aluminum hydroxide, antimony trioxide, perlite and kaolin.
[0009] The inventors added a fire-resistant, flame-retardant and heat-insulating agent composed of aluminum hydroxide, antimony trioxide, perlite and kaolin into the two-component fire-resistant, flame-retardant and heat-insulating coating, so that the two-component fire-resistant, flame-retardant and heat-insulating coating has certain fire-resistant, flame-retardant and heat-insulating effects.
[0010] Preferably, the weight ratio of aluminum hydroxide, antimony trioxide, perlite and kaolin in the fire-resistant flame retardant thermal insulation agent is 4-6:2-4:8-10:8-12.
[0011] Most preferably, the weight ratio of aluminum hydroxide, antimony trioxide, perlite and kaolin in the fire-resistant flame retardant thermal insulation agent is 5:3:9:10.
[0012] Preferably, the kaolin in the fire-resistant flame retardant heat insulating agent is modified kaolin.
[0013] Preferably, the modified kaolin is prepared by the following method:
[0014] (1) Add kaolin to water, then add barium chloride and sodium sulfate, stir ultrasonically for 1 to 2 hours, and filter to obtain a solid product;
[0015] (2) calcining the solid product at 1600-1700° C. for 2-4 hours, and obtaining a calcined product, i.e., the modified kaolin, after calcination.
[0016] The inventors surprisingly found through extensive research that the modified kaolin obtained by modifying the kaolin in the fire-resistant flame retardant and thermal insulation agent using the above method can significantly improve the fire-resistant flame retardant and thermal insulation effects of the two-component fire-resistant flame retardant and thermal insulation coating compared to the unmodified kaolin.
[0017] Further preferably, in step (1), the weight ratio of kaolin, barium chloride, sodium sulfate and water is 20-30:3-5:2.5-3.5:150-250;
[0018] Most preferably, in step (1), the weight ratio of kaolin, barium chloride, sodium sulfate and water is 25:4:3:200.
[0019] Preferably, in step (2), the solid product is calcined at 1680° C. for 3 h.
[0020] Further preferably, the modified kaolin further comprises step (3); the step (3) is:
[0021] (3) The calcined product is added to ethanol, and then a modifier is added. After stirring for 1 to 2 hours, the ethanol is evaporated to obtain the modified kaolin.
[0022] Preferably, the ethanol refers to an ethanol aqueous solution with a volume fraction of 50% to 95%;
[0023] Most preferably, the ethanol refers to an ethanol aqueous solution with a volume fraction of 70%.
[0024] More preferably, the modifier is pentaerythritol tetrastearate or sodium di(2-ethylhexyl)sulfosuccinate.
[0025] The inventors have further discovered through extensive research that modified kaolin obtained by further treating the calcined product with the above-mentioned modifier can further improve the fire retardant and heat insulating effects of the two-component fire-resistant, flame-retardant and heat-insulating coating.
[0026] Further preferably, the weight ratio of the calcined product, the modifier and the ethanol is 10-15:1-3:100;
[0027] Most preferably, the weight ratio of the calcined product, the modifier and ethanol is 13:2:100.
[0028] More preferably, the modifier consists of pentaerythritol tetrastearate and sodium di(2-ethylhexyl)sulfosuccinate.
[0029] The inventors further discovered in the study that the modified kaolin obtained by further treating the calcined product with a modifier consisting of pentaerythritol tetrastearate or sodium di(2-ethylhexyl) sulfonate can further improve the fire retardant and heat insulating effects of the two-component fire-resistant flame retardant and heat insulating coating; however, the degree of improvement is not large; the inventors surprisingly discovered in the study that the modified kaolin obtained by further treating the calcined product with a modifier consisting of pentaerythritol tetrastearate and sodium di(2-ethylhexyl) sulfonate can further significantly improve the fire retardant and heat insulating effects of the two-component fire-resistant flame retardant and heat insulating coating; the degree of improvement in the fire retardant and heat insulating effects of the two-component fire-resistant flame retardant and heat insulating coating is much higher than that of the modified kaolin obtained by further treating the calcined product with a single modifier pentaerythritol tetrastearate or a single sodium di(2-ethylhexyl) sulfonate.
[0030] More preferably, the weight ratio of pentaerythritol tetrastearate to sodium di(2-ethylhexyl)sulfosuccinate is 1-2:1-2.
[0031] Most preferably, the weight ratio of pentaerythritol tetrastearate to sodium di(2-ethylhexyl)sulfosuccinate is 1:1.
[0032] Preferably, the weight proportions of the water-based hydroxy resin, the additive, the fire-resistant flame retardant and the water in component A are respectively:
[0033] 80-100 parts of water-based hydroxy resin; 1-10 parts of additives; 30-50 parts of fire-resistant flame retardant and heat-insulating agent; 10-20 parts of water.
[0034] Preferably, the auxiliary agent consists of a wetting agent, a defoaming agent, a thickening agent, a coupling agent and a film-forming agent;
[0035] The weight ratio of the wetting agent, the defoaming agent, the thickener, the coupling agent and the film-forming agent is 1:1:1:1:4.
[0036] Preferably, the weight ratio of component A to component B is 3 to 10:1.
[0037] The present invention also provides an application of the two-component fire-resistant, flame-retardant and heat-insulating coating in automobile production.
[0038] Beneficial effects: The present invention provides a two-component fire-resistant flame retardant and thermal insulation coating prepared by a completely new method; the present invention adds a fire-resistant flame retardant and thermal insulation agent composed of aluminum hydroxide, antimony trioxide, perlite and kaolin into the two-component fire-resistant flame retardant and thermal insulation coating, so that the two-component fire-resistant flame retardant and thermal insulation coating has certain fire-resistant flame retardant and thermal insulation effects; in addition, the modified kaolin obtained by the method of the present invention is used in the fire-resistant flame retardant and thermal insulation agent, which can significantly improve the fire-resistant flame retardant and thermal insulation effects of the two-component fire-resistant flame retardant and thermal insulation coating compared with the use of unmodified kaolin. DETAILED DESCRIPTION
[0039] The present invention is further explained below in conjunction with specific examples, but the examples do not limit the present invention in any form.
[0040] The water-based hydroxylated acrylic emulsion in the following examples is a water-based hydroxylated acrylic emulsion of the brand LB-6019 of Lanbo. The remaining raw materials not specified are all conventional raw materials that can be purchased by those skilled in the art through conventional purchase channels or prepared by conventional methods.
[0041] Example 1 Preparation of two-component fire-resistant flame-retardant thermal insulation coating
[0042] The two-component fire-resistant, flame-retardant and heat-insulating coating is composed of component A and component B in a weight ratio of 5:1;
[0043] The B component is XP2655 curing agent;
[0044] The weight proportions of the component A are as follows: 90 parts of water-based hydroxy acrylic emulsion; 8 parts of auxiliary agent; 40 parts of fire-resistant flame retardant heat insulating agent; 15 parts of water;
[0045] The auxiliary agent is composed of a wetting agent, a defoamer, a thickener, a coupling agent and a film-forming agent in a weight ratio of 1:1:1:1:4; the wetting agent is the wetting agent BYK-346; the defoamer is the defoamer BYK-020; the thickener is the thickener SN-612; the coupling agent is the coupling agent Z-6011; and the film-forming agent is propylene glycol butyl ether;
[0046] The fire-resistant flame-retardant heat-insulating agent is a mixture of aluminum hydroxide, antimony trioxide, perlite and kaolin in a weight ratio of 5:3:9:10;
[0047] The preparation method of a two-component fire-resistant flame-retardant thermal insulation coating is as follows: a water-based hydroxy acrylic emulsion, an additive, a fire-resistant flame-retardant thermal insulation agent and water are mixed and dispersed evenly to obtain component A; component B is then added to component A and dispersed evenly to obtain the two-component fire-resistant flame-retardant thermal insulation coating.
[0048] Example 2 Preparation of two-component fire-resistant flame-retardant thermal insulation coating
[0049] The difference between Example 2 and Example 1 is that the fire-resistant flame retardant heat-insulating agent used in Example 2 is a modified fire-resistant flame retardant heat-insulating agent; the rest is the same as Example 1;
[0050] The modified kaolin is prepared by the following method:
[0051] (1) adding kaolin to water, followed by adding barium chloride and sodium sulfate, stirring for 1.5 hours under ultrasonic conditions, and filtering to obtain a solid product; wherein the weight ratio of kaolin, barium chloride, sodium sulfate and water is 25:4:3:200;
[0052] (2) calcining the solid product at 1680° C. for 3 h to obtain a calcined product, namely the modified kaolin.
[0053] Example 3 Preparation of two-component fire-resistant flame-retardant thermal insulation coating
[0054] The difference between Example 3 and Example 1 is that the fire-resistant flame retardant heat-insulating agent used in Example 3 is a modified fire-resistant flame retardant heat-insulating agent; the rest is the same as Example 1;
[0055] The modified kaolin is prepared by the following method:
[0056] (1) adding kaolin to water, followed by adding barium chloride and sodium sulfate, stirring for 1.5 hours under ultrasonic conditions, and filtering to obtain a solid product; wherein the weight ratio of kaolin, barium chloride, sodium sulfate and water is 25:4:3:200;
[0057] (2) calcining the solid product at 1680° C. for 3 h, and obtaining a calcined product after calcination;
[0058] (3) adding the calcined product into ethanol (70% by volume ethanol aqueous solution), then adding the modifier, stirring for 1.5 hours, and then evaporating the ethanol to obtain the modified kaolin;
[0059] In step (3), the weight ratio of the calcined product, the modifier and ethanol is 13:2:100; the modifier is pentaerythritol tetrastearate.
[0060] Example 4 Preparation of two-component fire-resistant flame-retardant thermal insulation coating
[0061] The difference between Example 4 and Example 1 is that the fire-resistant flame retardant heat-insulating agent used in Example 4 is a modified fire-resistant flame retardant heat-insulating agent; the rest is the same as Example 1;
[0062] The modified kaolin is prepared by the following method:
[0063] (1) adding kaolin to water, followed by adding barium chloride and sodium sulfate, stirring for 1.5 hours under ultrasonic conditions, and filtering to obtain a solid product; wherein the weight ratio of kaolin, barium chloride, sodium sulfate and water is 25:4:3:200;
[0064] (2) calcining the solid product at 1680° C. for 3 h, and obtaining a calcined product after calcination;
[0065] (3) adding the calcined product into ethanol (70% by volume ethanol aqueous solution), then adding the modifier, stirring for 1.5 hours, and then evaporating the ethanol to obtain the modified kaolin;
[0066] In step (3), the weight ratio of the calcined product, the modifier and ethanol is 13:2:100; the modifier is sodium di(2-ethylhexyl)sulfosuccinate.
[0067] Example 5 Preparation of two-component fire-resistant flame-retardant thermal insulation coating
[0068] The difference between Example 5 and Example 1 is that the fire-resistant flame retardant heat-insulating agent used in Example 5 is a modified fire-resistant flame retardant heat-insulating agent; the rest is the same as Example 1;
[0069] The modified kaolin is prepared by the following method:
[0070] (1) adding kaolin to water, followed by adding barium chloride and sodium sulfate, stirring for 1.5 hours under ultrasonic conditions, and filtering to obtain a solid product; wherein the weight ratio of kaolin, barium chloride, sodium sulfate and water is 25:4:3:200;
[0071] (2) calcining the solid product at 1680° C. for 3 h, and obtaining a calcined product after calcination;
[0072] (3) adding the calcined product into ethanol (70% by volume ethanol aqueous solution), then adding the modifier, stirring for 1.5 hours, and then evaporating the ethanol to obtain the modified kaolin;
[0073] In step (3), the weight ratio of the calcined product, the modifier and ethanol is 13:2:100; the modifier is composed of pentaerythritol tetrastearate and sodium di(2-ethylhexyl)sulfosuccinate in a weight ratio of 1:1.
[0074] The two-component fire-resistant flame-retardant heat-insulating coating prepared in Examples 1 to 5 was coated on a steel plate with a coating thickness of 150 μm; its fire resistance limit and thermal conductivity were tested; the test results are shown in Table 1;
[0075] Table 1. Performance test results of two-component fire-resistant flame-retardant thermal insulation coatings
[0076] Fire resistance Thermal conductivity Example 1 Two-component fire-resistant flame-retardant thermal insulation coating 61min 0.068W / (m·K) Example 2 Two-component fire-resistant flame-retardant thermal insulation coating 75min 0.051W / (m·K) Example 3 Two-component fire-resistant flame-retardant thermal insulation coating 84min 0.045W / (m·K) Example 4 Two-component fire-resistant flame-retardant thermal insulation coating 86min 0.044W / (m·K) Example 5 Two-component fire-resistant flame-retardant thermal insulation coating 111min 0.028W / (m·K)
[0077] It can be seen from the fire resistance limit time and thermal conductivity of Example 1 in Table 1 that the present invention can make the two-component fire-retardant and thermal insulation coating have certain fire-retardant and thermal insulation effects by adding a fire-retardant and thermal insulation agent composed of aluminum hydroxide, antimony trioxide, perlite and kaolin into the two-component fire-retardant and thermal insulation coating.
[0078] It can be seen from the experimental data in Table 1 that the two-component fire-resistant, flame-retardant and thermal insulation coating prepared in Example 2 has a fire resistance limit time significantly higher than that in Example 1, and a thermal conductivity significantly lower than that in Example 1; this indicates that adding modified kaolin obtained by modifying kaolin using the method described in the present invention to the fire-resistant, flame-retardant and thermal insulation coating can significantly improve the fire-resistant, flame-retardant and thermal insulation effects of the two-component fire-resistant, flame-retardant and thermal insulation coating compared to adding unmodified kaolin.
[0079] It can be seen from the experimental data in Table 1 that the two-component fire-resistant, flame-retardant and thermal insulation coatings prepared in Examples 3 and 4 have a fire resistance limit time that is further higher than that of Example 2, and at the same time, their thermal conductivity is further lower than that of Example 2; this indicates that in the preparation method of modified kaolin, the calcined product is further treated with a modifier, pentaerythritol tetrastearate or sodium di(2-ethylhexyl) sulfonate, to obtain a modified kaolin, compared to the modified kaolin not treated with pentaerythritol tetrastearate or sodium di(2-ethylhexyl) sulfonate, the fire retardant and thermal insulation effects of the two-component fire-resistant, flame-retardant and thermal insulation coatings can be further improved.
[0080] It can be seen from the experimental data in Table 1 that the two-component fire-resistant flame retardant and heat-insulating coating prepared in Example 4 has a fire resistance limit time that is much higher than that in Example 2, and is also much higher than that in Examples 3 and 4; its thermal conductivity is much lower than that in Example 2, and is also much lower than that in Examples 3 and 4; this shows that: the modified kaolin obtained by further treating the calcined product with a modifier pentaerythritol tetrastearate or sodium di(2-ethylhexyl) sulfonate can further improve the fire resistance and heat insulation effect of the two-component fire-resistant flame retardant and heat-insulating coating; however, its improvement The degree of improvement is not great; and the modified kaolin obtained by further treating the calcined product with a modifier composed of pentaerythritol tetrastearate and sodium di(2-ethylhexyl) sulfonate can further significantly improve the fire retardant and heat insulating effects of the two-component fire-resistant flame retardant thermal insulation coating; the degree of improvement in the fire retardant and heat insulating effects of the two-component fire-resistant flame retardant thermal insulation coating is much higher than that of the modified kaolin obtained by further treating the calcined product with a single modifier pentaerythritol tetrastearate or a single sodium di(2-ethylhexyl) sulfonate.
Claims
1. A two-component fire-resistant, flame-retardant and heat-insulating coating, comprising component A and component B; the component A comprises a water-based hydroxyl resin, an additive and water; the component B is a curing agent; characterized in that: The component A also contains a fire-resistant flame-retardant heat-insulating agent; The fire-resistant flame retardant heat-insulating agent comprises aluminum hydroxide, antimony trioxide, perlite and kaolin; the weight ratio of aluminum hydroxide, antimony trioxide, perlite and kaolin in the fire-resistant flame retardant heat-insulating agent is 4-6:2-4:8-10:8-12; The kaolin described in the fire-resistant flame retardant heat insulating agent is modified kaolin; the modified kaolin is prepared by the following method: (1) Add kaolin to water, then add barium chloride and sodium sulfate, stir under ultrasonic conditions for 1-2 hours, and filter to obtain a solid product; (2) calcining the solid product at 1600-1700°C for 2-4 hours, and obtaining a calcined product after calcination; (3) adding the calcined product to ethanol, then adding a modifier, stirring for 1 to 2 hours, and then evaporating the ethanol to obtain the modified kaolin; the modifier is composed of pentaerythritol tetrastearate and sodium di(2-ethylhexyl) sulfonate succinate; the weight ratio of pentaerythritol tetrastearate to sodium di(2-ethylhexyl) sulfonate succinate is 1 to 2:1 to 2; In step (1), the weight ratio of kaolin, barium chloride, sodium sulfate and water is 20-30:3-5:2.5-3.5:150-250; The weight proportions of water-based hydroxy resin, auxiliary agent, fire-resistant flame retardant heat insulating agent and water in component A are respectively: 80-100 parts of water-based hydroxy resin; 1-10 parts of auxiliary agent; 30-50 parts of fire-resistant flame retardant heat insulating agent; and 10-20 parts of water.
2. The two-component fire-resistant, flame-retardant and heat-insulating coating according to claim 1, characterized in that: The weight ratio of aluminum hydroxide, antimony trioxide, perlite and kaolin in the fire-resistant flame retardant thermal insulation agent is 5:3:9:
10.
3. The two-component fire-resistant, flame-retardant and heat-insulating coating according to claim 1, characterized in that: In step (1), the weight ratio of kaolin, barium chloride, sodium sulfate and water is 25:4:3:
200.
4. The two-component fire-resistant, flame-retardant and heat-insulating coating according to claim 1, characterized in that: In step (2), the solid product is calcined at 1680° C. for 3 h.
5. The two-component fire-resistant, flame-retardant and heat-insulating coating according to claim 1, characterized in that: The weight ratio of component A to component B is 3~10:
1.
6. Use of the two-component fire-resistant, flame-retardant and heat-insulating coating according to any one of claims 1 to 5 in automobile production.