High-thermal-conductivity silicone rubber material and preparation method thereof

By adding modified silicone rubber, alumina, sulfur-containing flame retardant and other components to the silicone rubber material, the thermal conductivity of carbon nanotubes and boron nitride is solved, and the problem of insufficient thermal conductivity of existing silicone rubber materials is achieved. The high thermal conductivity and flame retardant effect are improved significantly, and the overall performance of the material is greatly improved.

CN118895048AInactive Publication Date: 2024-11-05DONGGUAN GENDIAN NEW MATERIAL CO LTD

Patent Information

Application Number
CN202410945814.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing silicone rubber materials have shortcomings in thermal conductivity, which has failed to effectively improve their thermal conductivity, and the flame retardant performance has not been fully improved.

Method used

Modified silicone rubber, silicone rubber, alumina, sulfur-containing flame retardant, hydroxylated boron nitride and zinc chloride are blended through a twin-screw extruder to prepare high-thermal conductivity silicone rubber materials, using carbon nanotubes and sulfur-containing flame retardants improve the thermal conductivity and flame retardant properties of the material.

Benefits of technology

The flame retardant and thermal conductivity of high-thermal conductivity silicone rubber materials have been achieved, which significantly improves the ultimate oxygen index and combustion grade of the material, while improving the thermal conductivity coefficient and enhancing the overall performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of silicone rubber, and discloses a high-thermal-conductivity silicone rubber material and a preparation method thereof.The high-thermal-conductivity silicone rubber material is obtained by adding modified silicone rubber, silicone rubber, aluminum oxide, a sulfur-containing flame retardant, hydroxylated boron nitride and zinc chloride into a double-screw extruder, blending and extruding. Carbon nanotubes in the modified silicone rubber have flame retardant property and high heat-conducting property, sulfur element in the sulfur-containing flame retardant can promote the carbonization process of the material during combustion, and a formed carbon layer can effectively block oxygen and heat, so that the flame retardant property of the material is improved; the carbon nanotubes are easy to agglomerate, and the agglomeration of the carbon nanotubes is reduced by modifying the carbon nanotubes, so that the heat conduction effect of the carbon nanotubes is better; the modified silicone rubber and the silicone rubber have good compatibility, and the compatibility between the carbon nanotubes and the silicone rubber is improved at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicone rubber, in particular to a high thermal conductivity silicone rubber material and a preparation method thereof. Background Art

[0002] Silicone rubber is a polymer compound composed of oxygen atoms and silicon atoms, and has good cold resistance, heat resistance and chemical corrosion resistance. It has good elasticity and maintains its physical properties over a wide temperature range. For example, patent CN112679960 discloses a method for preparing a high-temperature resistant flame-retardant silicone rubber material. The present invention has effectively improved the existing method for preparing silicone rubber materials, so that flame-retardant fillers and modified vinyl polydimethylsiloxane are efficiently and stably combined with methyl vinyl silicone rubber, so that the influence of additives on the mechanical properties of silicone rubber is minimized. The prepared high-temperature resistant flame-retardant silicone rubber material has high flame retardant properties; however, its thermal conductivity is not improved. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies in the prior art, the present invention provides a high thermal conductivity silicone rubber material and a preparation method thereof, which has good flame retardant and thermal conductive effects.

[0005] (II) Technical solution

[0006] To achieve the above object, the present invention provides the following technical solution: a high thermal conductivity silicone rubber material, comprising the following weight components: 8-12 parts by weight of modified silicone rubber, 80-100 parts by weight of silicone rubber, 4-6 parts by weight of aluminum oxide, 2-4 parts by weight of sulfur-containing flame retardant, 1-2 parts by weight of hydroxylated boron nitride, and 2-4 parts by weight of zinc chloride;

[0007] The preparation method of the sulfur-containing flame retardant is as follows: 6-8 parts by weight of the intermediate 1 is added to an N,N-dimethylamide solvent, and the mixture is stirred and dispersed, and then 1-2 parts by weight of a benzoin dimethyl ether photoinitiator and 5-9 parts by weight of aminoethanethiol are added thereto, and the mixture is irradiated with 365 nm ultraviolet light at 20-30° C. for 2-3 hours, and the mixture is centrifuged, washed with deionized water, and dried to obtain the sulfur-containing flame retardant.

[0008] Preferably, the preparation method of the modified silicone rubber is:

[0009] (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, stirring to dissolve, reacting at 85-90° C. for 5-10 hours, washing, filtering and drying after the reaction, to obtain tertiary aminomaleopimaric acid;

[0010] (2) Add tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, stir and disperse, react at 90-105° C. for 8-14 hours, filter after reaction, and dry to obtain intermediate 1;

[0011] (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid thereto, reacting at 85-110° C. for 7-15 hours, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2;

[0012] (4) Add intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, react at 80-110° C. for 10-14 hours, and then wash and dry to obtain modified silicone rubber.

[0013] Preferably, the mass ratio of maleopimaric acid to dimethylaminopropylamine in (1) is 1:1.1-1.3.

[0014] Preferably, the mass ratio of tertiary aminomaleopimaric acid to 6-chloro-1-hexene in (2) is 1:0.8-1.2.

[0015] Preferably, the mass ratio of the hydroxylated carbon nanotubes, the intermediate 1, and p-toluenesulfonic acid in (3) is 1.2-1.5:1:0.01-0.03.

[0016] Preferably, the mass ratio of the intermediate 2, hydrogen-containing silicone oil and platinum catalyst in (4) is 1:1.2-1.4:0.02-0.04.

[0017] Preferably, the preparation method of the high thermal conductivity silicone rubber material is: adding modified silicone rubber, silicone rubber, alumina, sulfur-containing flame retardant, hydroxylated boron nitride, and zinc chloride into a twin-screw extruder, with a blending temperature of 185-195°C and an extrusion temperature of 170-180°C to obtain a high thermal conductivity silicone rubber material.

[0018] (III) Beneficial technical effects

[0019] The invention obtains the high thermal conductive silicone rubber material by adding modified silicone rubber, silicone rubber, aluminum oxide, sulfur-containing flame retardant, hydroxylated boron nitride and zinc chloride into a twin-screw extruder, blending and extruding.

[0020] The anhydride group of maleopimaric acid and the amino group of dimethylaminopropylamine are reacted to obtain tertiary amino maleopimaric acid, thereby introducing a tertiary amine group into the maleopimaric acid; then the X group thereof and the X group of 6-chloro-1-hexene are reacted to introduce an olefin group to obtain an intermediate 1; the hydroxylated carbon nanotube and the intermediate 1 are subjected to an esterification reaction under the action of p-toluenesulfonic acid to obtain an intermediate 2; the intermediate 2, hydrogen-containing silicone oil and a platinum catalyst are added into a reactor to react to obtain a modified silicone rubber; the intermediate 1 and aminoethanethiol are subjected to an addition reaction to obtain a sulfur-containing flame retardant.

[0021] The carbon nanotubes in the modified silicone rubber have flame retardant properties and high thermal conductivity. The sulfur element in the sulfur-containing flame retardant can promote the carbonization process of the material when burning, and the formed carbon layer can effectively block oxygen and heat, thereby improving the flame retardant property of the material. The thermal conductivity coefficients of the boron nitride and the carbon nanotubes contained in the present invention are both large, and have good thermal conductivity. Adding them to the silicone rubber material improves its thermal conductivity. The carbon nanotubes are easy to agglomerate, and modifying them also reduces their agglomeration, thereby improving their thermal conductivity. The modified silicone rubber has good compatibility with silicone rubber, and the compatibility between the carbon nanotubes and silicone rubber is improved. DETAILED DESCRIPTION

[0022] Preparation of hydroxylated carbon nanotubes: 0.3 g of carbon nanotubes were added into concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for acidification to obtain hydroxylated carbon nanotubes.

[0023] Example 1

[0024] (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, wherein the mass ratio of maleopimaric acid to dimethylaminopropylamine is 1:1.1, stirring to dissolve, reacting at 85° C. for 5 h, washing, filtering and drying after completion, to obtain tertiary aminomaleopimaric acid;

[0025] (2) adding tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, wherein the mass ratio of tertiary amino maleopimaric acid to 6-chloro-1-hexene is 1:0.8, stirring and dispersing, reacting at 90° C. for 8 h, filtering after completion, and drying to obtain intermediate 1;

[0026] (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid, wherein the mass ratio of hydroxylated carbon nanotubes, intermediate 1, and p-toluenesulfonic acid is 1.2:1:0.01, reacting at 85° C. for 7 h, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2;

[0027] (4) adding intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, wherein the mass ratio of intermediate 2, hydrogen-containing silicone oil and platinum catalyst is 1:1.2:0.02, reacting at 80° C. for 10 h, washing and drying after completion, to obtain modified silicone rubber;

[0028] (5) adding 6 parts by weight of the intermediate 1 to an N,N-dimethylamide solvent, stirring and dispersing, adding 1 part by weight of benzoin dimethyl ether photoinitiator and 5 parts by weight of aminoethanethiol, irradiating with 365 nm ultraviolet light at 20° C. for 2 h, centrifuging, washing with deionized water, and drying to obtain a sulfur-containing flame retardant;

[0029] (6) 8 parts by weight of modified silicone rubber, 80 parts by weight of silicone rubber, 4 parts by weight of aluminum oxide, 2 parts by weight of sulfur-containing flame retardant, 1 part by weight of hydroxylated boron nitride, and 2 parts by weight of zinc chloride are added into a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 170° C. to obtain a high thermal conductive silicone rubber material.

[0030] Example 2

[0031] (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, wherein the mass ratio of maleopimaric acid to dimethylaminopropylamine is 1:1.3, stirring to dissolve, reacting at 90° C. for 10 h, washing, filtering and drying after completion, to obtain tertiary aminomaleopimaric acid;

[0032] (2) adding tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, wherein the mass ratio of tertiary amino maleopimaric acid to 6-chloro-1-hexene is 1:1.2, stirring and dispersing, reacting at 105° C. for 14 h, filtering after completion, and drying to obtain intermediate 1;

[0033] (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid, wherein the mass ratio of hydroxylated carbon nanotubes, intermediate 1, and p-toluenesulfonic acid is 1.5:1:0.03, reacting at 110° C. for 15 h, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2;

[0034] (4) adding intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, wherein the mass ratio of intermediate 2, hydrogen-containing silicone oil and platinum catalyst is 1:1.4:0.04, reacting at 110° C. for 14 h, washing and drying after completion, to obtain modified silicone rubber;

[0035] (5) adding 8 parts by weight of the intermediate 1 to an N,N-dimethylamide solvent, stirring and dispersing, adding 2 parts by weight of benzoin dimethyl ether photoinitiator and 9 parts by weight of aminoethanethiol, irradiating with 365 nm ultraviolet light at 30° C. for 3 h, centrifuging, washing with deionized water, and drying to obtain a sulfur-containing flame retardant;

[0036] (6) 12 parts by weight of modified silicone rubber, 100 parts by weight of silicone rubber, 6 parts by weight of aluminum oxide, 4 parts by weight of sulfur-containing flame retardant, 2 parts by weight of hydroxylated boron nitride, and 4 parts by weight of zinc chloride are added into a twin-screw extruder at a blending temperature of 195° C. and an extrusion temperature of 180° C. to obtain a high thermal conductive silicone rubber material.

[0037] Example 3

[0038] (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, wherein the mass ratio of maleopimaric acid to dimethylaminopropylamine is 1:1.2, stirring to dissolve, reacting at 87° C. for 7.5 h, washing, filtering and drying after completion, to obtain tertiary aminomaleopimaric acid;

[0039] (2) adding tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, wherein the mass ratio of tertiary amino maleopimaric acid to 6-chloro-1-hexene is 1:1.0, stirring and dispersing, reacting at 100° C. for 11 h, filtering after completion, and drying to obtain intermediate 1;

[0040] (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid, wherein the mass ratio of hydroxylated carbon nanotubes, intermediate 1, and p-toluenesulfonic acid is 1.35:1:0.02, reacting at 97° C. for 11 h, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2;

[0041] (4) adding intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, wherein the mass ratio of intermediate 2, hydrogen-containing silicone oil and platinum catalyst is 1:1.3:0.03, reacting at 95° C. for 12 h, washing and drying after completion, to obtain modified silicone rubber;

[0042] (5) adding 7 parts by weight of the intermediate 1 to an N,N-dimethylamide solvent, stirring and dispersing, adding 1.5 parts by weight of benzoin dimethyl ether photoinitiator and 7 parts by weight of aminoethanethiol, irradiating with 365 nm ultraviolet light at 25° C. for 2.5 h, centrifuging, washing with deionized water, and drying to obtain a sulfur-containing flame retardant;

[0043] (6) 10 parts by weight of modified silicone rubber, 90 parts by weight of silicone rubber, 5 parts by weight of aluminum oxide, 3 parts by weight of sulfur-containing flame retardant, 1.5 parts by weight of hydroxylated boron nitride, and 3 parts by weight of zinc chloride are added into a twin-screw extruder at a blending temperature of 190° C. and an extrusion temperature of 175° C. to obtain a high thermal conductive silicone rubber material.

[0044] Example 4

[0045] (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, wherein the mass ratio of maleopimaric acid to dimethylaminopropylamine is 1:1.1, stirring to dissolve, reacting at 85° C. for 5 h, washing, filtering and drying after completion, to obtain tertiary aminomaleopimaric acid;

[0046] (2) adding tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, wherein the mass ratio of tertiary amino maleopimaric acid to 6-chloro-1-hexene is 1:0.8, stirring and dispersing, reacting at 90° C. for 8 h, filtering after completion, and drying to obtain intermediate 1;

[0047] (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid, wherein the mass ratio of hydroxylated carbon nanotubes, intermediate 1, and p-toluenesulfonic acid is 1.5:1:0.03, reacting at 110° C. for 15 h, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2;

[0048] (4) adding intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, wherein the mass ratio of intermediate 2, hydrogen-containing silicone oil and platinum catalyst is 1:1.4:0.04, reacting at 110° C. for 14 h, washing and drying after completion, to obtain modified silicone rubber;

[0049] (5) adding 7 parts by weight of the intermediate 1 to an N,N-dimethylamide solvent, stirring and dispersing, adding 1.5 parts by weight of benzoin dimethyl ether photoinitiator and 7 parts by weight of aminoethanethiol, irradiating with 365 nm ultraviolet light at 25° C. for 2.5 h, centrifuging, washing with deionized water, and drying to obtain a sulfur-containing flame retardant;

[0050] (6) 10 parts by weight of modified silicone rubber, 90 parts by weight of silicone rubber, 5 parts by weight of aluminum oxide, 3 parts by weight of sulfur-containing flame retardant, 1.5 parts by weight of hydroxylated boron nitride, and 3 parts by weight of zinc chloride are added into a twin-screw extruder at a blending temperature of 190° C. and an extrusion temperature of 175° C. to obtain a high thermal conductive silicone rubber material.

[0051] Example 5

[0052] (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, wherein the mass ratio of maleopimaric acid to dimethylaminopropylamine is 1:1.3, stirring to dissolve, reacting at 90° C. for 10 h, washing, filtering and drying after completion, to obtain tertiary aminomaleopimaric acid;

[0053] (2) adding tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, wherein the mass ratio of tertiary amino maleopimaric acid to 6-chloro-1-hexene is 1:1.2, stirring and dispersing, reacting at 105° C. for 14 h, filtering after completion, and drying to obtain intermediate 1;

[0054] (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid, wherein the mass ratio of hydroxylated carbon nanotubes, intermediate 1, and p-toluenesulfonic acid is 1.35:1:0.02, reacting at 97° C. for 11 h, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2;

[0055] (4) adding intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, wherein the mass ratio of intermediate 2, hydrogen-containing silicone oil and platinum catalyst is 1:1.3:0.03, reacting at 95° C. for 12 h, washing and drying after completion, to obtain modified silicone rubber;

[0056] (5) adding 6 parts by weight of the intermediate 1 to an N,N-dimethylamide solvent, stirring and dispersing, adding 1 part by weight of benzoin dimethyl ether photoinitiator and 5 parts by weight of aminoethanethiol, irradiating with 365 nm ultraviolet light at 20° C. for 2 h, centrifuging, washing with deionized water, and drying to obtain a sulfur-containing flame retardant;

[0057] (6) 8 parts by weight of modified silicone rubber, 80 parts by weight of silicone rubber, 4 parts by weight of aluminum oxide, 2 parts by weight of sulfur-containing flame retardant, 1 part by weight of hydroxylated boron nitride, and 2 parts by weight of zinc chloride are added into a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 170° C. to obtain a high thermal conductive silicone rubber material.

[0058] Comparative Example 1

[0059] (1) adding 6 parts by weight of the intermediate 1 to an N,N-dimethylamide solvent, stirring and dispersing, adding 1 part by weight of benzoin dimethyl ether photoinitiator and 5 parts by weight of aminoethanethiol, irradiating with 365 nm ultraviolet light at 20° C. for 2 h, centrifuging, washing with deionized water, and drying to obtain a sulfur-containing flame retardant;

[0060] (2) 80 parts by weight of silicone rubber, 4 parts by weight of aluminum oxide, 2 parts by weight of a sulfur-containing flame retardant, 1 part by weight of hydroxylated boron nitride, and 2 parts by weight of zinc chloride are added to a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 170° C. to obtain a high thermal conductive silicone rubber material.

[0061] Comparative Example 2

[0062] (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, wherein the mass ratio of maleopimaric acid to dimethylaminopropylamine is 1:1.3, stirring to dissolve, reacting at 90° C. for 10 h, washing, filtering and drying after completion, to obtain tertiary aminomaleopimaric acid;

[0063] (2) adding tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, wherein the mass ratio of tertiary amino maleopimaric acid to 6-chloro-1-hexene is 1:1.2, stirring and dispersing, reacting at 105° C. for 14 h, filtering after completion, and drying to obtain intermediate 1;

[0064] (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid, wherein the mass ratio of hydroxylated carbon nanotubes, intermediate 1, and p-toluenesulfonic acid is 1.35:1:0.02, reacting at 97° C. for 11 h, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2;

[0065] (4) adding intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, wherein the mass ratio of intermediate 2, hydrogen-containing silicone oil and platinum catalyst is 1:1.3:0.03, reacting at 95° C. for 12 h, washing and drying after completion, to obtain modified silicone rubber;

[0066] (5) 8 parts by weight of modified silicone rubber, 80 parts by weight of silicone rubber, 4 parts by weight of aluminum oxide, 1 part by weight of hydroxylated boron nitride, and 2 parts by weight of zinc chloride are added into a twin-screw extruder at a blending temperature of 185° C. and an extrusion temperature of 170° C. to obtain a high thermal conductive silicone rubber material.

[0067] The limiting oxygen index of the material was tested using an oxygen index meter, and the combustion grade of the material was tested using a horizontal and vertical combustion instrument. The test results are shown in Table 1.

[0068] Table 1: Flame retardancy tests.

[0069] project Limiting oxygen index (%) Combustion level Example 1 30 V-0 Example 2 33 V-0 Example 3 32 V-0 Example 4 28 V-0 Example 5 29 V-0 Comparative Example 1 21 V-1 Comparative Example 2 20 V-1

[0070] It can be seen from Table 1 that Examples 1-5 of the present invention have better flame retardant effects than Comparative Examples 1-2.

[0071] The thermal conductivity test was carried out with reference to GB / T 22588-2008 “Flash method for measuring thermal diffusivity or thermal conductivity”. The test results are shown in Table 2.

[0072] Table 2: Thermal conductivity test.

[0073] project Thermal conductivity (W / m·K) Example 1 5.32 Example 2 5.49 Example 3 5.31 Example 4 5.24 Example 5 5.37 Comparative Example 1 3.12 Comparative Example 2 4.35

[0074] It can be seen from Table 2 that Examples 1-5 of the present invention have better thermal conductivity than Comparative Examples 1-2.

[0075] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A high thermal conductivity silicone rubber material, It is characterized in that The invention comprises the following components by weight: 8-12 parts by weight of modified silicone rubber, 80-100 parts by weight of silicone rubber, 4-6 parts by weight of aluminum oxide, 2-4 parts by weight of sulfur-containing flame retardant, 1-2 parts by weight of hydroxylated boron nitride, and 2-4 parts by weight of zinc chloride; The preparation method of the sulfur-containing flame retardant is as follows: 6-8 parts by weight of the intermediate 1 is added to an N,N-dimethylamide solvent, and the mixture is stirred and dispersed, and then 1-2 parts by weight of a benzoin dimethyl ether photoinitiator and 5-9 parts by weight of aminoethanethiol are added thereto, and the mixture is irradiated with 365 nm ultraviolet light at 20-30° C. for 2-3 hours, and the mixture is centrifuged, washed with deionized water, and dried to obtain the sulfur-containing flame retardant.

2. The high thermal conductivity silicone rubber material according to claim 1, It is characterized in that The preparation method of the modified silicone rubber is: (1) adding maleopimaric acid and dimethylaminopropylamine to an ethanol solvent, stirring to dissolve, reacting at 85-90° C. for 5-10 hours, washing, filtering and drying after the reaction, to obtain tertiary aminomaleopimaric acid; (2) Add tertiary amino maleopimaric acid and 6-chloro-1-hexene to a flask containing acetonitrile solvent, stir and disperse, react at 90-105° C. for 8-14 hours, filter after reaction, and dry to obtain intermediate 1; (3) Adding hydroxylated carbon nanotubes and intermediate 1 to N,N-dimethylformamide solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid thereto, reacting at 85-110° C. for 7-15 hours, and then distilling under reduced pressure, washing with deionized water, and drying to obtain intermediate 2; (4) Add intermediate 2, hydrogen-containing silicone oil and platinum catalyst into a reaction kettle, react at 80-110° C. for 10-14 hours, and then wash and dry to obtain modified silicone rubber.

3. The high thermal conductivity silicone rubber material according to claim 2, It is characterized in that The mass ratio of maleopimaric acid to dimethylaminopropylamine in (1) is 1:1.1-1.

3.

4. The high thermal conductivity silicone rubber material according to claim 2, It is characterized in that The mass ratio of tertiary amino maleopimaric acid to 6-chloro-1-hexene in (2) is 1:0.8-1.

2.

5. The high thermal conductivity silicone rubber material according to claim 2, It is characterized in that The mass ratio of the hydroxylated carbon nanotubes, the intermediate 1 and p-toluenesulfonic acid in (3) is 1.2-1.5:1:0.01-0.

03.

6. The high thermal conductivity silicone rubber material according to claim 2, It is characterized in that The mass ratio of the intermediate 2, hydrogen-containing silicone oil and platinum catalyst in (4) is 1:1.2-1.4:0.02-0.

04.

7. A method for preparing the high thermal conductivity silicone rubber material according to any one of claims 1 to 6, It is characterized in that The preparation method of the high thermal conductivity silicone rubber material is: adding modified silicone rubber, silicone rubber, aluminum oxide, sulfur-containing flame retardant, hydroxylated boron nitride and zinc chloride into a twin-screw extruder, with a blending temperature of 185-195° C. and an extrusion temperature of 170-180° C. to obtain the high thermal conductivity silicone rubber material.

Citation Information

Patent Citations

  • Heat-conducting insulating silicone rubber for 5G and preparation method of heat-conducting insulating silicone rubber

    CN113897062A

  • Preparation and application of functionally modified heat-conducting silicone rubber material

    CN115124847A

Cited By

  • Silicone rubber for brain-computer interface and preparation method thereof

    CN119752189A