Polyimide precursor composition, polyimide film, and polyimide film / substrate laminate

By using a polyimide precursor composition with a moderate imidization rate and heat treatment technology, a polyimide film with excellent thermal properties and transparency is formed, which solves the problems of existing polyimide films in terms of thermal properties and transparency. The lack of transparency meets the high performance requirements of flexible electronic devices.

CN116457211BActive Publication Date: 2024-10-29UBE CORPORATION
View PDF 22 Cites 0 Cited by

Patent Information

Application Number
CN202180078956.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-10-29
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

Existing polyimide films have deficiencies in thermal properties, heat resistance, and transparency, making it difficult to meet the needs of high-performance flexible electronic devices.

Method used

A polyimide precursor composition with an imidization rate between 0% and 50%, including specific repeating units and a solvent, is used to form a polyimide film through an imidization reaction, and is carried out on a glass substrate Heat treatment to form a polyimide film/substrate laminate, further forming conductor and semiconductor layers on the laminate, and finally peeling off the substrate to produce a flexible electronic device.

Benefits of technology

It achieves low linear thermal expansion coefficient, excellent transparency and high heat resistance, and is suitable for the manufacture of high-performance flexible electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116457211B_ABST
    Figure CN116457211B_ABST
Patent Text Reader

Abstract

Provided is a polyimide precursor composition capable of manufacturing a polyimide film having excellent thermal properties and / or heat resistance and excellent transparency. The polyimide precursor composition comprises: a polyimide precursor, wherein the repeating unit is composed of a repeating unit represented by the following general formula (I) and a repeating unit of the general formula (I) that is further imidized, and the imidization rate is greater than 0% and less than 50%; and a solvent. (In the general formula I, more than 70 mol% of X1 is a structure represented by the formula (1-1):, and more than 70 mol% of Y1 is a structure represented by the formula (D-1) and / or (D-2).)#imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyimide precursor composition suitable for use in electronic devices such as substrates of flexible devices, a polyimide film having improved properties, and a polyimide film / substrate laminate, and also relates to a method for producing a flexible electronic device using the composition. Background Art

[0002] Polyimide films are widely used in the fields of electrical / electronic devices, semiconductors, etc. due to their excellent heat resistance, chemical resistance, mechanical strength, electrical properties, dimensional stability, etc. On the other hand, in recent years, with the advent of a highly information-based society, the development of optical materials such as optical fibers and optical waveguides in the field of optical communications, and liquid crystal alignment films and protective films for color filters in the field of display devices is being promoted. In particular, in the field of display devices, as a substitute for glass substrates, research on lightweight and highly flexible plastic substrates and the development of displays that can be bent or rolled up are being actively carried out.

[0003] In displays such as liquid crystal displays and organic EL displays, semiconductor elements such as TFTs are formed to drive each pixel. Therefore, heat resistance and dimensional stability are required for the substrate. Polyimide films are expected to be used as substrates for display applications due to their excellent heat resistance, chemical resistance, mechanical strength, electrical properties, dimensional stability, etc.

[0004] Polyimide is generally colored yellow-brown, and therefore its use in transmissive devices such as liquid crystal displays with backlights is limited. However, in recent years, polyimide films having excellent transparency in addition to mechanical and thermal properties have been developed, and expectations for their use as substrates for display applications have further increased (see Patent Documents 1 to 3).

[0005] Generally, it is difficult to maintain the planarity of a flexible film, and therefore it is difficult to uniformly and accurately form semiconductor elements such as TFTs, fine wiring, etc. on the flexible film. For example, Patent Document 4 describes "a method for manufacturing a flexible device as a display device or a light receiving device, which includes the following steps: a step of applying a specific precursor resin composition to a carrier substrate and forming a film to form a solid polyimide resin film; a step of forming a circuit on the resin film; and a step of peeling the solid resin film with the circuit formed on the surface from the carrier substrate."

[0006] In addition, Patent Document 5 discloses a method for manufacturing a flexible device, which includes: after forming components and circuits required for the device on a polyimide film / glass substrate laminate obtained by forming a polyimide film on a glass substrate, irradiating the glass substrate with laser from the glass substrate side to peel off the glass substrate.

[0007] Patent document 6 discloses a polyimide precursor composition, which contains a polyimide precursor composition in which one of a tetracarboxylic acid component and a diamine component is a compound having an alicyclic structure, and the other contains a repeating unit from a compound having an aromatic ring, and an imidazole compound; and a method of manufacturing a polyimide film / glass substrate laminate using the polyimide precursor composition. The polyimide film obtained by the invention of patent document 6 has a small thickness direction phase difference (retardation), excellent mechanical properties, and excellent transparency.

[0008] In addition, Patent Document 7 describes a polyimide precursor having an imidization rate of 30 mol% or more and 90 mol% or less obtained from a tetracarboxylic acid and a specific diamine compound (see Claim 1). When the polyimide precursor is used to produce a polyimide film, an advantageous effect of reducing the linear thermal expansion coefficient can be obtained without resorting to the stretching operation often performed in the production of polyfilms.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: International Publication No. 2012 / 011590

[0012] Patent Document 2: International Publication No. 2013 / 179727

[0013] Patent Document 3: International Publication No. 2014 / 038715

[0014] Patent Document 4: Japanese Patent Application Publication No. 2010-202729

[0015] Patent Document 5: International Publication No. 2018 / 221607

[0016] Patent Document 6: International Publication No. 2015 / 080158

[0017] Patent Document 7: International Publication No. 2014 / 067079 Summary of the invention

[0018] Problems to be solved by the invention

[0019] As described above, the invention of Patent Document 7 enables production of a polyimide film having excellent properties, and various properties such as thermal properties, heat resistance, mechanical properties, and transparency are expected to be further improved in a balanced manner.

[0020] The present invention is made in view of the existing problems, and its main purpose is to provide a polyimide precursor composition capable of producing a polyimide film having excellent thermal properties and / or heat resistance and excellent transparency. In addition, one embodiment of the present invention aims to provide a polyimide film and a polyimide film / substrate laminate obtained using the polyimide precursor composition, and further, another embodiment of the present invention aims to provide a method for producing a flexible electronic device using the polyimide precursor composition and a flexible electronic device.

[0021] Means for solving problems

[0022] The main disclosures of this application are summarized as follows

[0023] 1. A polyimide precursor composition, characterized in that it contains:

[0024] A polyimide precursor, wherein the repeating unit is composed of a repeating unit represented by the following general formula (I) and a repeating unit of the general formula (I) that is further imidized, and the imidization rate is more than 0% and less than 50%; and

[0025] Solvent.

[0026] [Chemistry 1]

[0027]

[0028] (In the general formula I, X1 is a tetravalent aliphatic group or an aromatic group, Y1 is a divalent aliphatic group or an aromatic group, R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms, wherein 70 mol% or more of X1 is of the formula (1-1):

[0029] [Chemistry 2]

[0030]

[0031] The structure shown in FIG. 1 , 70 mol % or more of Y1 is of formula (D-1) and / or (D-2):

[0032] [Chemistry 3]

[0033]

[0034] The structure shown.)

[0035] 2. The polyimide precursor composition according to item 1 above, wherein a polyimide film obtained from the polyimide precursor composition has a light transmittance of 79% or more at a wavelength of 400 nm in the case of a film having a thickness of 10 μm.

[0036] 3. The polyimide precursor composition according to item 1 or 2 above, wherein a polyimide film obtained from the polyimide precursor composition has a linear thermal expansion coefficient of 20 ppm / K or less at 150° C. to 250° C. in the case of a film having a thickness of 10 μm.

[0037] 4. The polyimide precursor composition according to any one of items 1 to 3 above, wherein a polyimide obtained from the polyimide precursor composition has a 5% weight loss temperature of 500° C. or higher.

[0038] 5. The polyimide precursor composition according to any one of items 1 to 4 above, wherein a polyimide film obtained from the polyimide precursor composition has a breaking elongation of 10% or more in the case of a film having a thickness of 10 μm.

[0039] 6. The polyimide precursor composition according to any one of the above items 1 to 5, wherein 90 mol % or more of X1 is a structure represented by the above formula (1-1).

[0040] 7. A polyimide film obtained from the polyimide precursor composition according to any one of items 1 to 6 above.

[0041] 8. A polyimide film / substrate laminate, characterized in that it has:

[0042] A polyimide film obtained from the polyimide precursor composition described in any one of items 1 to 6 above; and

[0043] Base material.

[0044] 9. The laminate according to item 8 above, wherein the base material is a glass substrate.

[0045] 10. A method for producing a polyimide film / substrate laminate, comprising:

[0046] (a) a step of applying the polyimide precursor composition described in any one of items 1 to 6 above onto a substrate; and

[0047] (b) A step of heat-treating the polyimide precursor on the substrate to form a polyimide film on the substrate.

[0048] 11. The production method according to item 10 above, wherein the substrate is a glass substrate.

[0049] 12. A method for manufacturing a flexible electronic device, comprising:

[0050] (a) a step of applying the polyimide precursor composition described in any one of items 1 to 6 above onto a substrate;

[0051] (b) a step of heat-treating the polyimide precursor on the substrate to produce a polyimide film / substrate laminate having a polyimide film laminated on the substrate;

[0052] (c) forming at least one layer selected from a conductor layer and a semiconductor layer on the polyimide film of the laminate; and

[0053] (d) A step of peeling the substrate and the polyimide film.

[0054] 13. The production method according to item 12 above, wherein the substrate is a glass substrate.

[0055] Effects of the Invention

[0056] According to the present invention, a polyimide precursor composition can be provided, which can produce a polyimide film having excellent thermal properties (low linear thermal expansion coefficient, etc.) and / or heat resistance (5% weight loss temperature, etc.) and excellent transparency. According to an embodiment of the polyimide precursor composition of the present invention, it is possible to produce a polyimide film having at least one of (i) thermal properties such as a low linear thermal expansion coefficient and (ii) heat resistance such as a 5% weight loss temperature and excellent transparency.

[0057] Furthermore, according to one embodiment of the present invention, a polyimide film and a polyimide film / substrate laminate obtained using the polyimide precursor composition can be provided. Furthermore, according to another embodiment of the present invention, a method for producing a flexible electronic device using the polyimide precursor composition and a flexible electronic device can be provided. DETAILED DESCRIPTION

[0058] In the present application, "flexible (electronic) device" means that the device itself is flexible, and usually, a semiconductor layer (transistors, diodes, etc. as components) is formed on a substrate to complete the device. "Flexible (electronic) device" is different from existing devices such as COF (Chip On Film) that have "hard" semiconductor components such as IC chips mounted on FPC (flexible printed circuit board). However, in order to operate or control the "flexible (electronic) device" of the present application, there is no problem in mounting "hard" semiconductor components such as IC chips on a flexible substrate, or electrically connecting them, or fusing them for use. As preferred flexible (electronic) devices, there can be cited display devices such as liquid crystal displays, organic EL displays, and electronic paper, solar cells, and light receiving devices such as CMOS.

[0059] Hereinafter, the polyimide precursor composition of the present invention will be described, and then the method for producing a flexible electronic device will be described.

[0060] <<Polyimide Precursor Composition>>

[0061] The polyimide precursor composition for forming a polyimide film contains a polyimide precursor and a solvent. The polyimide precursor is dissolved in the solvent.

[0062] The polyimide precursor contains a repeating unit represented by the following general formula (I) and a repeating unit obtained by further imidizing the general formula (I).

[0063] [Chemistry 4]

[0064]

[0065] (In general formula I, X1 is a tetravalent aliphatic group or an aromatic group, Y1 is a divalent aliphatic group or an aromatic group, and R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms.)

[0066] The repeating unit of the general formula (I) which is further imidized means a structure in which one or both of the two amide bonds present in the general formula (I) are converted into imide bonds, and specifically, is represented by the following general formulae (Ib), (Ic) and (II).

[0067] [Chemistry 5]

[0068]

[0069] [Chemistry 6]

[0070]

[0071] [Chemistry 7]

[0072]

[0073] The imidization rate refers to the ratio of the amide bond in the general formula (I) to the imide bond. Therefore, when all repeating units in the polyimide precursor are of the general formula (I), the imidization rate is 0%, when all repeating units are of the general formula (Ib) and / or (Ic), the imidization rate is 50%, and if all repeating units are of the general formula (II), the imidization rate is 100% (i.e., polyimide). In the present invention, the imidization rate is greater than 0% and less than 50%, which means that in addition to the structure of the general formula (I), one or more of the general formulas (Ib), (Ic) and (II) are present in a manner to achieve a specified imidization rate.

[0074] The imidization rate can be used to measure the polyimide precursor (solution). 1 The H-NMR spectrum was calculated from the ratio of the integrated value of the peak of aromatic protons (7 to 8.3 ppm) to the integrated value of the peak of amide protons (9.5 to 10.5 ppm).

[0075] In addition, the polyimide precursor with adjusted imidization rate can be produced by the following production method, which includes the following steps: when the tetracarboxylic acid component and the diamine component react, or after obtaining a precursor having a repeating unit represented by the general formula (I) from the tetracarboxylic acid component and the diamine component, reacting for an appropriate time under appropriate conditions for the imidization reaction in a manner to achieve the desired imidization rate.

[0076] As described in detail later, the method can be roughly divided into: a method in which the imidization reaction is carried out evenly (or randomly) in the molecule (for the sake of convenience, it is called a one-stage supply method); and a method in which the tetracarboxylic acid component and the diamine component are separately supplied and the imidization reaction is carried out only between a part of the tetracarboxylic acid component and a part of the diamine component (or in blocks) (for the sake of convenience, it is called a multi-stage supply method).

[0077] In the one-stage supply method, when the tetracarboxylic acid component and the diamine component react, or after the precursor having the repeating unit shown in the general formula (I) is obtained from the tetracarboxylic acid component and the diamine component, the reaction is carried out at an appropriate temperature for an appropriate time so that the imidization is carried out to the target imidization rate. As a temperature range, for example, it is above 0°C, preferably above 15°C, for example, below 180°C, preferably below 150°C, and more preferably below 130°C. As a time range, generally, the higher the temperature, the shorter the time it is possible to adjust the imidization rate, and the lower the temperature, the longer the time it is possible to adjust the imidization rate, for example, preferably in a range of more than a few seconds, for example, more than 1 minute to about 1 year or less. In addition, the reaction temperature and reaction time are also preferably changed according to the presence or absence, type, and amount of the imidazole compound added later. The one-stage supply method is preferably implemented by thermal imidization, preferably without including a dehydrating agent for chemical imidization.

[0078] In the two-stage supply method, the tetracarboxylic acid component and the diamine component are separately supplied to multiple steps, and the imidization rate is adjusted by reacting under different conditions in multiple steps. As an example of the two-stage supply, the following method is used: in the first step, only a part of the tetracarboxylic acid component and a part of the diamine component are supplied, including high-temperature heating in which the imidization reaction proceeds rapidly, and as a result, a precursor of complete imidization or high imidization rate is obtained, and then the remaining tetracarboxylic acid component and diamine component are supplied in the second step, and the reaction is carried out under conditions in which the imidization reaction is suppressed. The high-temperature heating conditions of the first step are preferably 100°C or more, more preferably 120°C to 250°C, and the temperature conditions of the second step are less than 100°C, more preferably less than 90°C. It is usually 0°C or more, preferably 15°C or more. The imidization rate can be adjusted by the distribution ratio of the tetracarboxylic acid component and the diamine component in the first step and the second step. In this method, it is also preferably implemented by thermal imidization, and it is preferably not included in the dehydrating agent used for chemical imidization.

[0079] The general formulae (Ib), (Ic) and (II) are repeating units in which the structure of the general formula (I) is further imidized, and therefore X1, Y1, R1 and R2 in the general formulae (Ib), (Ic) and (II) may be groups derived from the general formula (I). Therefore, the description of the preferred structure of the general formula (I) below also applies to the structures of the general formulae (Ib), (Ic) and (II).

[0080] The precursor represented by the general formula (I) is particularly preferably a polyamic acid in which R1 and R2 are hydrogen atoms. When X1 and Y1 are aliphatic groups, the aliphatic group is preferably a group having an alicyclic structure.

[0081] In all repeating units in the polyimide precursor, preferably 70 mol% or more of X1 is a structure represented by the following formula (1-1), i.e., a structure derived from norbornane-2-spiro-α-cyclopentanone-α′-spiro-2″-norbornane-5,5″,6,6″-tetracarboxylic dianhydride (hereinafter abbreviated as CpODA as needed).

[0082] [Chemistry 8]

[0083]

[0084] In all repeating units in the polyimide precursor, preferably 70 mol% or more of Y1 is a structure represented by the following formula (D-1) and / or (D-2), that is, a structure derived from 4,4′-diaminobenzanilide (abbreviated to DABAN as needed).

[0085] [Chemistry 9]

[0086]

[0087] By using a composition containing such a polyimide precursor, a polyimide film having excellent thermal characteristics such as a low linear thermal expansion coefficient and excellent transparency can be produced.

[0088] The polyimide precursor will be described using monomers (tetracarboxylic acid component, diamine component, and other components) that provide X1 and Y1 in the general formula (I), and then the production method will be described.

[0089] In this specification, tetracarboxylic acid component includes tetracarboxylic acid, tetracarboxylic dianhydride, and tetracarboxylic acid derivatives such as tetracarboxylic acid silyl ester, tetracarboxylic ester, and tetracarboxylic acid chloride used as raw materials for manufacturing polyimide. Although not particularly limited, it is simple to use tetracarboxylic dianhydride in manufacturing. In the following description, the example of using tetracarboxylic dianhydride as tetracarboxylic acid component is described. In addition, diamine component is a diamine compound with 2 amino groups (-NH2) used as raw materials for manufacturing polyimide.

[0090] In addition, in this specification, the polyimide film refers to both the film formed on the (carrier) substrate and present in the laminate, and the film after peeling off the substrate. In addition, the material obtained by heat-treating (imidizing) the material constituting the polyimide film, that is, the polyimide precursor composition, is sometimes referred to as "polyimide material".

[0091] <X1 and tetracarboxylic acid component>

[0092] As described above, in all the repeating units in the polyimide precursor, preferably 70 mol% or more of X1 has the structure represented by the formula (1-1), more preferably 80 mol% or more, still more preferably 90 mol% or more, and most preferably 95 mol% or more (also very preferably 100 mol%) has the structure represented by the formula (1-1). The tetracarboxylic dianhydride that provides the structure of formula (1-1) for X1 is CpODA.

[0093] CpODA can be a mixture of spatial isomers, or can also be a specific spatial isomer. There is no particular limitation. As preferred spatial isomers, trans-endo-endo-norbornane-2-spiro-α-cyclopentanone-α'-spiro-2”-norbornane-5,5”,6,6”-tetracarboxylic dianhydride (CpODA-tee) and cis-endo-endo-norbornane-2-spiro-α-cyclopentanone-α'-spiro-2”-norbornane-5,5”,6,6”-tetracarboxylic dianhydride (CpODA-cee) can be cited.

[0094] [Chemical formula 10]

[0095]

[0096] In a preferred embodiment, in CpODA, at least 50 mol% or more, and still more preferably 63 mol% or more is CpODA-tee. In another preferred embodiment, in CpODA, at least 30 mol% or more, and still more preferably 37 mol% or more is CpODA-cee. In yet another preferred embodiment, in CpODA, the total of CpODA-tee and CpODA-cee is at least 80 mol% or more, and still more preferably 83 mol% or more.

[0097] In the present invention, a tetravalent aliphatic group or aromatic group (abbreviated as "other X1") other than the structure represented by the formula (1-1) can be contained in an amount within a range that does not impair the effects of the present invention as X1. That is, in addition to CpODA, the tetracarboxylic acid component can contain other tetracarboxylic acid derivatives in an amount within a range that does not impair the effects of the present invention. Relative to 100 mol% of the tetracarboxylic acid component, the amount of other tetracarboxylic acid derivatives is less than 30 mol%, more preferably less than 20 mol%, still more preferably less than 10 mol% (also preferably 0 mol%).

[0098] When "other X1" is a tetravalent group having an aromatic ring, it is preferably a tetravalent group having 6 to 40 carbon atoms and having an aromatic ring.

[0099] Examples of the tetravalent group having an aromatic ring include the following groups.

[0100] [Chemistry 11]

[0101]

[0102] (In the formula, Z1 is a direct bond or any of the following divalent groups.

[0103] [Chemistry 12]

[0104]

[0105] Wherein, Z2 in the formula is a divalent organic group, Z3 and Z4 are each independently an amide bond, an ester bond, or a carbonyl bond, and Z5 is an organic group containing an aromatic ring.

[0106] Specific examples of Z2 include an aliphatic hydrocarbon group having 2 to 24 carbon atoms and an aromatic hydrocarbon group having 6 to 24 carbon atoms.

[0107] Specific examples of Z5 include aromatic hydrocarbon groups having 6 to 24 carbon atoms.

[0108] As the tetravalent group having an aromatic ring, the following tetravalent groups are particularly preferred because the obtained polyimide film can have both high heat resistance and high transparency.

[0109] [Chemistry 13]

[0110]

[0111] (Wherein, Z1 is a direct bond or a hexafluoroisopropylidene bond.)

[0112] Here, Z1 is more preferably a direct bond because the obtained polyimide film can achieve high heat resistance, high transparency, and a low linear thermal expansion coefficient.

[0113] In addition, as a preferred group, in the above formula (9), Z1 can be exemplified as the following formula (3A):

[0114] [Chemistry 14]

[0115]

[0116] The compound containing the fluorenyl group shown. 11 and Z 12 Each of them is independently preferably the same and is a single bond or a divalent organic group.11 and Z 12 , preferably an organic group containing an aromatic ring, preferably a structure represented by formula (3A1).

[0117] [Chemistry 15]

[0118]

[0119] (Z 13 and Z 14 are independently a single bond, -COO-, -OCO- or -O-, where Z 14 When it is bonded to a fluorenyl group, Z is preferably 13 is -COO-, -OCO- or -O- and Z 14 It is a single bond structure; R 91 is an alkyl group or a phenyl group having 1 to 4 carbon atoms, preferably a methyl group, and n is an integer of 0 to 4, preferably 1.

[0120] Examples of the tetracarboxylic acid component providing a repeating unit of the general formula (I) in which X1 is a tetravalent group having an aromatic ring include 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, pyromellitic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2, 3,3',4'-biphenyltetracarboxylic acid, 4,4'-oxydiphthalic acid, bis(3,4-dicarboxyphenyl)sulfone, m-terphenyl-3,4,3',4'-tetracarboxylic acid, p-terphenyl-3,4,3',4'-tetracarboxylic acid, dicarboxyphenyldimethylsilane, dicarboxyphenoxydiphenyl sulfide, sulfonyldiphthalic acid, tetracarboxylic acid dianhydride, tetracarboxylic acid silyl ester, tetracarboxylic acid ester, tetracarboxylic acid chloride and other derivatives thereof. As the tetracarboxylic acid component providing a repeating unit of the general formula (I) in which X1 is a tetravalent group having an aromatic ring containing a fluorine atom, for example, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, tetracarboxylic acid dianhydride, tetracarboxylic acid silyl ester, tetracarboxylic acid ester, tetracarboxylic acid chloride and other derivatives thereof can be cited. Furthermore, as a preferred compound, (9H-fluorene-9,9-diyl)bis(2-methyl-4,1-phenylene)bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylate) can be mentioned. The tetracarboxylic acid component may be used alone or in combination of two or more.

[0121] When "other X1" is a tetravalent group having an alicyclic structure, it is preferably a tetravalent group having an alicyclic structure having 4 to 40 carbon atoms, more preferably having at least one aliphatic 4-12-membered ring, more preferably an aliphatic 4-membered ring or an aliphatic 6-membered ring. Examples of the tetravalent group having a preferred aliphatic 4-membered ring or aliphatic 6-membered ring include the following groups.

[0122] [Chemistry 16]

[0123]

[0124] (Where R 31 ~R 38 Each independently represents a direct bond or a divalent organic group. 41 ~R 47 , and R 71 ~R 73 Each independently represents one selected from the group consisting of groups represented by the formula: -CH2-, -CH=CH-, -CH2CH2-, -O-, and -S-. 48 is an organic group containing an aromatic ring or an alicyclic structure.

[0125] As R 31 , R 32 , R 33 , R 34 , R 35 , R 36 , R 37 , R 38 Specifically, there can be mentioned a direct bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, an oxygen atom (—O—), a sulfur atom (—S—), a carbonyl bond, an ester bond, and an amide bond.

[0126] As R 48 Examples of the aromatic ring-containing organic group include the following groups.

[0127] [Chemistry 17]

[0128]

[0129] (W1 is a direct bond or a divalent organic group, n 11 ~n 13 Each independently represents an integer from 0 to 4, R 51 , R 52 , R 53 Each is independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group, or a trifluoromethyl group.)

[0130] Specific examples of W1 include a direct bond, a divalent group represented by the following formula (5), and a divalent group represented by the following formula (6).

[0131] [Chemistry 18]

[0132]

[0133] (R in formula (6) 61 ~R68 Each independently represents a direct bond or any one of the divalent groups represented by the above formula (5).

[0134] As the tetravalent group having an alicyclic structure, the following groups are particularly preferred because the resulting polyimide can have high heat resistance, high transparency, and a low linear thermal expansion coefficient.

[0135] [Chemistry 19]

[0136]

[0137] As the tetracarboxylic acid component that provides the repeating unit of formula (I) in which X1 is a tetravalent group having an alicyclic structure, examples thereof include 1,2,3,4-cyclobutanetetracarboxylic acid, isopropylidenediphenoxybisphthalic acid, cyclohexane-1,2,4,5-tetracarboxylic acid, [1,1'-bi(cyclohexane)]-3,3',4,4'-tetracarboxylic acid, [1,1'-bi(cyclohexane)]-2,3,3',4'-tetracarboxylic acid, [1,1'-bi(cyclohexane)]-2,2',3,3'-tetracarboxylic acid, 4,4'-methylenebis(cyclohexane-1,2-dicarboxylic acid), 4,4'-(propane-2,2-diyl)bis(cyclohexane-1,2-dicarboxylic acid), 4,4'-oxybis(cyclohexane-1,2-dicarboxylic acid), 4,4'-thiobis(cyclohexane-1,2-dicarboxylic acid), 4,4'-sulfonylbis(cyclohexane-1,2-dicarboxylic acid), 4,4'-(dimethylsilanediyl)bis(cyclohexane-1,2-dicarboxylic acid), 4,4'-(tetrafluoropropane-2,2-diyl)bis(cyclohexane-1,2-dicarboxylic acid), octahydrobicyclopentadiene-1,3,4,6-tetracarboxylic acid, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic acid, 6-(carboxymethyl)bicyclo[2.2.1]heptane-2,3,5-tricarboxylic acid, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic acid, bicyclo[2.2.2]oct-5-ene-2,3,7,8-tetracarboxylic acid, tricyclo[4.2.2.02,5]decane-3,4,7,8-tetracarboxylic acid, tricyclo[4.2.2.02,5]dec-7-ene-3,4,9,10-tetracarboxylic acid, 9-oxatricyclo[4.2.1.02,5]nonane-3,4,7,8-tetracarboxylic acid, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethanonaphthalene-2c,3c,6c,7c-tetracarboxylic acid, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethanonaphthalene-2t,3t,6c,7c-tetracarboxylic acid, decahydro-1,4-ethano-5,8-methanonaphthalene-2,3,6,7-tetracarboxylic acid, tetradecahydro-1,4:5,8:9,10-trimethanoanthracene-2,3,6,7-tetracarboxylic acid, and derivatives thereof such as their tetracarboxylic dianhydrides, tetracarboxylic silyl esters, tetracarboxylic esters, and tetracarboxylic acid chlorides. The tetracarboxylic acid component may be used alone, or two or more thereof may be used in combination.

[0138] <Y1 and diamine component>

[0139] As described above, among all repeating units in the polyimide precursor, Y1 preferably has a structure represented by formula (D-1) and / or (D-2) in an amount of 70 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more (preferably 100 mol%) or more. The diamine compound that provides the structure of formula (D-1) or formula (D-2) as Y1 is 4,4'-diaminobenzanilide (abbreviated as DABAN).

[0140] In the present invention, a divalent aliphatic group or aromatic group other than the structures represented by formula (D-1) and (D-2) (abbreviated as "other Y1") can be contained as Y1 in an amount within a range that does not impair the effect of the present invention. That is, in addition to DABAN, the diamine component can contain other diamine compounds in an amount within a range that does not impair the effect of the present invention. The amount of the other diamine compound is less than 30 mol%, more preferably less than 20 mol%, and even more preferably less than 10 mol% (also preferably 0 mol%) relative to 100 mol% of the diamine component.

[0141] When "other Y1" is a divalent group having an aromatic ring, it is preferably a divalent group having 6 to 40 carbon atoms, more preferably a divalent group having 6 to 20 carbon atoms.

[0142] Examples of the divalent group having an aromatic ring include the following groups.

[0143] [Chemistry 20]

[0144]

[0145] (W1 is a direct bond or a divalent organic group, n 11 ~n 13 Each independently represents an integer from 0 to 4, R 51 , R 52 , R 53 Each is independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group, or a trifluoromethyl group.)

[0146] Specific examples of W1 include a direct bond, a divalent group represented by the following formula (5), and a divalent group represented by the following formula (6).

[0147] [Chemistry 21]

[0148]

[0149] [Chemistry 22]

[0150]

[0151] (R in formula (6) 61 ~R68 Each independently represents a direct bond or any one of the divalent groups represented by the above formula (5).

[0152] Here, since the obtained polyimide can take into account high heat resistance, high transparency, and low linear thermal expansion coefficient, W1 is particularly preferably a direct bond or one selected from the group consisting of groups represented by the formula: -NHCO-, -CONH-, -COO-, and -OCO-. In addition, W1 is also particularly preferably R 61 ~R 68 Any of the divalent groups represented by the above formula (6) which is a direct bond or one selected from the group consisting of groups represented by the formula: -NHCO-, -CONH-, -COO-, and -OCO-. When -NHCO- or -CONH- is selected, "other Y1" is selected in a manner different from that of formula (D-1) or formula (D-2).

[0153] In addition, as a preferred group, in the above formula (4), W1 can be exemplified as the following formula (3B):

[0154] [Chemistry 23]

[0155]

[0156] The fluorene group compound shown. 11 and Z 12 Each of them is independently preferably the same and is a single bond or a divalent organic group. 11 and Z 12 , preferably an organic group containing an aromatic ring, preferably a structure represented by formula (3B1).

[0157] [Chemistry 24]

[0158]

[0159] (Z 13 and Z 14 are independently a single bond, -COO-, -OCO- or -O-, where Z 14 When it is bonded to a fluorenyl group, Z is preferably 13 is -COO-, -OCO- or -O- and Z 14 It is a single bond structure; R 91 is an alkyl group having 1 to 4 carbon atoms or a phenyl group, preferably a phenyl group, and n is an integer of 0 to 4, preferably 1. )

[0160] As other preferred groups, in the above formula (4), compounds in which W1 is a phenylene group, that is, terphenylenediamine compounds can be mentioned, and compounds in which all of them are bonded at the para position are particularly preferred.

[0161] As other preferred groups, in the above formula (4), W1 can be exemplified as R in the structure where the first phenyl ring of formula (6) is 61 and R 62 A 2,2-propylene compound.

[0162] As another preferred group, in the above formula (4), there can be mentioned a compound where W1 is represented by the following formula (3B2).

[0163] [Chemistry 25]

[0164]

[0165] Examples of the diamine component providing a repeating unit of the general formula (I) in which Y1 is a divalent group having an aromatic ring include p-phenylenediamine, m-phenylenediamine, benzidine, 3,3'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, m-tolidine, 3,4'-diaminobenzanilide, N,N'-bis(4-aminophenyl)terephthalamide, N,N'-p-phenylenebis(p-aminobenzamide), 4-aminophenoxy-4-diaminobenzoate, bis(4-aminophenyl)-p-phenylenebis(p-aminobenzamide), dicarboxylate, biphenyl-4,4'-dicarboxylic acid bis(4-aminophenyl) ester, p-phenylene bis(p-aminobenzoate), bis(4-aminophenyl)-[1,1'-biphenyl]-4,4'-dicarboxylate, [1,1'-biphenyl]-4,4'-diylbis(4-aminobenzoate), 4,4'-oxydiphenylamine, 3,4'-oxydiphenylamine, 3,3'-oxydiphenylamine, p-methylenebis(phenylenediamine), 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy) Benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, bis(4-aminophenyl)sulfone, 3,3'-bis(trifluoromethyl)benzidine, 3,3'-bis((aminophenoxy)phenyl)propane, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(4-(4-aminophenoxy)diphenyl)sulfone, bis(4-(3-aminophenoxy)diphenyl) Sulfone, octafluorobenzidine, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 2,4-bis(4-aminoanilino)-6-amino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-methylamino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-ethylamino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-anilino-1,3,5-triazine. Examples of the diamine component providing a repeating unit of the general formula (I) in which Y1 is a divalent group having an aromatic ring containing a fluorine atom include 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, and 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.Preferred diamine compounds include 9,9-bis(4-aminophenyl)fluorene, 4,4'-(((9H-fluorene-9,9-diyl)bis([1,1'-biphenyl]-5,2-diyl))bis(oxy))diamine, [1,1':4',1"-terphenyl]-4,4"-diamine, and 4,4'-([1,1'-binaphthyl]-2,2'-diylbis(oxy))diamine. The diamine components may be used alone or in combination of two or more.

[0166] When "other Y1" is a divalent group having an alicyclic structure, it is preferably a divalent group having an alicyclic structure having 4 to 40 carbon atoms, more preferably having at least one aliphatic 4- to 12-membered ring, and more preferably an aliphatic 6-membered ring.

[0167] Examples of the divalent group having an alicyclic structure include the following groups.

[0168] [Chemistry 26]

[0169]

[0170] (wherein, V1 and V2 are each independently a direct bond or a divalent organic group, n 21 ~n 26 Each independently represents an integer from 0 to 4, R 81 ~R 86 are each independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group, or a trifluoromethyl group, R 91 , R 92 , R 93 Each is independently selected from the group consisting of groups represented by the formula: -CH2-, -CH=CH-, -CH2CH2-, -O-, -S-.)

[0171] Specific examples of V1 and V2 include a direct bond and a divalent group represented by the above formula (5).

[0172] As the divalent group having an alicyclic structure, the following groups are particularly preferred because the resulting polyimide can have both high heat resistance and a low linear thermal expansion coefficient.

[0173] [Chemistry 27]

[0174]

[0175] As the divalent group having an alicyclic structure, the following groups are preferred.

[0176] [Chemistry 28]

[0177]

[0178] Examples of the diamine component providing a repeating unit of the general formula (I) in which Y1 is a divalent group having an alicyclic structure include 1,4-diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-2-ethylcyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,4-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-tert ... cyclobutane, 1,4-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, diaminobicycloheptane, diaminomethylbicycloheptane, diaminooxybicycloheptane, diaminomethoxybicycloheptane, isophoronediamine, diaminotricyclodecane, diaminomethyltricyclodecane, bis(aminocyclohexyl)methane, bis(aminocyclohexyl)isopropylidene, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane. The diamine components may be used alone or in combination of two or more.

[0179] As the tetracarboxylic acid component and the diamine component providing the repeating unit represented by the general formula (I), any of aliphatic tetracarboxylic acids other than alicyclic ones (particularly dianhydrides) and / or aliphatic diamines can be used, and the content thereof is preferably less than 30 mol%, more preferably less than 20 mol%, and further preferably less than 10 mol% (including 0%) relative to 100 mol% of the total of the tetracarboxylic acid component and the diamine component.

[0180] By containing a structure represented by formula (4) as "other Y1", or by containing a diamine compound such as p-phenylenediamine, 3,3'-bis(trifluoromethyl)benzidine, m-tolidine, or 4,4'-bis(4-aminophenoxy)biphenyl as a specific compound, the transparency of the obtained polyimide film can sometimes be improved. In addition, by containing a structure represented by formula (3B) as "other Y1", or by containing a diamine compound such as 9,9-bis(4-aminophenyl)fluorene as a specific compound, Tg can sometimes be increased and the phase difference (retardation) in the film thickness direction can be reduced.

[0181] The polyimide precursor can be prepared from the above-mentioned tetracarboxylic acid component and diamine component. According to the chemical structure taken by R1 and R2, the polyimide precursor used in the present invention (including at least one of the repeating units represented by the above formula (I)) can be classified as follows:

[0182] 1) Polyamic acid (R1 and R2 are hydrogen; also known as polyamic acid);

[0183] 2) Polyamic acid ester (at least a part of R1 and R2 is an alkyl group; also known as polyamic acid ester);

[0184] 3) 4) Polyamic acid silyl ester (at least a part of R1 and R2 is an alkylsilyl group; also known as polyamic acid silyl ester).

[0185] And the polyimide precursor can be easily produced by the following production method according to this classification. However, the production method of the polyimide precursor used in the present invention is not limited to the following production method.

[0186] 1) Polyamic acid

[0187] When the repeating unit represented by formula (I) is a polyamic acid, any of the following methods can be adopted: a one-stage supply method in which the imidization reaction is carried out evenly (or randomly) within the molecule; and a multi-stage supply method in which the tetracarboxylic acid component and the diamine component are separately supplied and the imidization reaction is carried out only between a part of the tetracarboxylic acid component and a part of the diamine component (or in blocks).

[0188] The manufacturing example of the polyimide precursor based on the one-stage supply method is described. In a solvent, tetracarboxylic dianhydride and diamine components as tetracarboxylic acid components are reacted at a relatively low temperature of, for example, 120°C or less while suppressing excessive imidization in a roughly equimolar ratio, preferably a molar ratio of diamine component to tetracarboxylic acid component [number of moles of diamine component / number of moles of tetracarboxylic acid component] of 0.90 to 1.10, and more preferably 0.95 to 1.05. There is no limitation, more specifically, diamine is dissolved in an organic solvent or water, tetracarboxylic dianhydride is slowly added to the solution while stirring, and stirred for 1 to 72 hours in the range of 0 to 120°C, preferably 5 to 80°C. In addition, thereafter, it can also be stored at 5°C to 40°C for a specified time, such as 1 day to 1 year, for example, and further imidization is carried out to adjust the imidization rate. The order of addition of diamine and tetracarboxylic dianhydride is easy to increase the molecular weight of the polyimide precursor, so it is preferred. In addition, the order of adding the diamine and tetracarboxylic dianhydride in the above-mentioned manufacturing method can also be reversed, which is preferred because the precipitate is reduced. When water is used as a solvent, it is preferred to add an imidazole such as 1,2-dimethylimidazole or a base such as triethylamine in an amount of 0.8 times or more of the carboxyl group of the generated polyamic acid (polyimide precursor).

[0189] When the reaction of the tetracarboxylic acid component and the diamine component is carried out at a relatively high temperature, for example, at a temperature above 80°C, above 90°C, or above 100°C, the target imidization rate can be achieved in a relatively short time while suppressing excessive imidization reaction, and thus it can be directly used as the "polyimide precursor composition of the present invention".

[0190] On the other hand, the temperature (heating) stage (stage) of the reaction can also be divided into two stages. In one embodiment, in the first stage, the reaction of the tetracarboxylic acid component and the diamine component is carried out at a relatively low temperature (e.g., 0°C or more, for example, 80°C or less, and then 70°C or less), to obtain a polyimide precursor with a low imidization rate (including an imidization rate of 0%), and then in the second stage, at a relatively high temperature, for example, 80°C or more, preferably 90°C or more, and more preferably 100°C or more, for example, heating for 5 minutes to 72 hours, it is possible to achieve a target imidization rate while suppressing excessive imidization reaction. In addition, in different embodiments, the reaction of the tetracarboxylic acid component and the diamine component can be carried out at a relatively low temperature (e.g., 0°C or more, such as 80°C or less, and further 70°C or less) in the first stage to obtain a polyimide precursor with a low imidization rate (including an imidization rate of 0%), and then in the second stage, imidization is carried out at a relatively low temperature, such as 0°C or more and 80°C or less (or less than 80°C), preferably 70°C or less, for a predetermined time, such as about 1 day to 1 year, thereby adjusting the imidization rate. If the temperature (heating) stage of the reaction is divided into two stages, it is advantageous that in the first stage, a stable polymerization reaction can be carried out by carrying out the reaction of the tetracarboxylic acid component and the diamine component at a relatively low temperature.

[0191] Next, for the production example of the polyimide precursor based on the multi-stage supply method, the two-stage supply is used as an example to illustrate. First, in the first step, under the conditions of the imidization reaction, specifically, for example, at a temperature of 100°C or above, tetracarboxylic dianhydride as a tetracarboxylic acid component and a diamine component are reacted. More specifically, the diamine is dissolved in a solvent, and the tetracarboxylic dianhydride is slowly added to the solution while stirring, and stirred at 100°C or above, preferably in the range of 120 to 250°C for 0.5 to 72 hours, thereby obtaining a soluble imide compound. The order of adding the diamine and the tetracarboxylic dianhydride can also be reversed.

[0192] The degree of polymerization of the imide compound can be determined by the molar ratio of the tetracarboxylic acid component and the diamine component to be reacted so as to make the imide compound soluble. Both ends of the soluble imide compound may be an acid anhydride group or a carboxyl group, or may be an amino group.

[0193] Imidization is performed by thermal imidization, so no chemical imidization agent is used. Here, the chemical imidization agent refers to an acid anhydride (dehydrating agent) such as acetic anhydride and an amine compound (catalyst) such as pyridine and isoquinoline.

[0194] Next, in the second step, a tetracarboxylic acid component and / or a diamine component are added to the reaction solution containing the soluble imide compound obtained in the first step to react and obtain the polyimide precursor of the present invention. In the second step, the tetracarboxylic acid component and / or the diamine component are added so that the molar ratio of the total amount of the tetracarboxylic acid component and the total amount of the diamine component reacted in the first step and the second step is approximately equimolar, preferably the molar ratio of the diamine component to the tetracarboxylic acid component [the number of moles of the diamine component / the number of moles of the tetracarboxylic acid component] is 0.90 to 1.10, more preferably 0.95 to 1.05.

[0195] In the second step, the reaction is carried out under conditions that suppress imidization, specifically, at a temperature of less than 100°C. More specifically, a diamine is added to the reaction solution containing a soluble imide compound obtained in the first step, and the mixture is stirred for 1 to 72 hours at a temperature less than 100°C, preferably in the range of -20 to 80°C, and then tetracarboxylic dianhydride is added, and the mixture is stirred for 1 to 72 hours at a temperature less than 100°C, preferably in the range of -20 to 80°C. The polyimide precursor of the present invention is obtained. The order of adding the diamine and the tetracarboxylic dianhydride may be reversed, and the diamine and the tetracarboxylic dianhydride may be added simultaneously. In addition, when the total amount of the tetracarboxylic acid component to be reacted is added to the solvent in the first step, only the diamine is added, and when the total amount of the diamine component to be reacted is added to the solvent in the first step, only the tetracarboxylic dianhydride is added.

[0196] Imidization can also be carried out in the second step, but the reaction temperature and reaction time are appropriately selected so that the imidization rate of the polyimide precursor finally obtained is within a specified range. In this way, the imidization rate can be adjusted by mainly generating repeating units of an imide structure (structure of general formula (II)) in the first step and mainly generating repeating units of an amic acid structure represented by the above chemical formula (I) in the second step.

[0197] 2) Polyamic acid ester

[0198] When the repeating unit shown in formula (I) is a polyamic acid ester, it is obtained by the following reaction. First, tetracarboxylic dianhydride is reacted with any alcohol to obtain a dicarboxylic acid diester, and then reacted with a chlorinating agent (thionyl chloride, oxalyl chloride, etc.) to obtain a diester dicarboxylic acid chloride. The diester dicarboxylic acid chloride and diamine are stirred at -20 to 120 ° C, preferably in the range of -5 to 80 ° C for 1 to 72 hours to obtain a polyimide precursor (polyamic acid ester). In the case of reacting above 80 ° C, the molecular weight varies depending on the temperature history during polymerization, and imidization is performed by heat, so it is possible that a polyimide precursor cannot be stably manufactured. In addition, by using a phosphorus-based condensing agent, a carbodiimide condensing agent, etc. to dehydrate and condense a dicarboxylic acid diester and a diamine, a polyimide precursor can also be easily obtained.

[0199] Since the polyimide precursor obtained by this method is stable, it can also be purified by adding a solvent such as water or alcohol and performing reprecipitation.

[0200] The obtained polyimide precursor (polyamic acid ester) can be reacted in the same manner as the item 1) of the polyamic acid (refer to the one-stage supply method, i.e., the first stage temperature is low-the second stage temperature is high and the first stage temperature is low-the second stage temperature is low). That is, in a certain embodiment, heating at a relatively high temperature, for example, 80°C or more, preferably 90°C or more, and more preferably 100°C or more, for example, for 5 minutes to 72 hours, can achieve the target imidization rate while suppressing excessive imidization reaction. In addition, in another embodiment, imidization can also be carried out at a relatively low temperature, for example, 0°C or more and 80°C or less (or less than 80°C), preferably 70°C or less, for a specified time, for example, 1 day to 1 year, to adjust the imidization rate.

[0201] 3) Polyamic acid silyl ester (indirect method)

[0202] When the repeating unit shown in formula (I) is a polyamic acid silyl ester, it is obtained by the indirect method described in this item or the direct method described in the next item. First, in the indirect method, a diamine is reacted with a silylating agent in advance to obtain a silylated diamine. The silylated diamine is purified by distillation or the like as needed. Then, the silylated diamine is dissolved in a dehydrated solvent in advance, and tetracarboxylic dianhydride is slowly added while stirring, and stirred at 0 to 120° C., preferably in the range of 5 to 80° C. for 1 to 72 hours, thereby obtaining a polyimide precursor. In the case of a reaction above 80° C., the molecular weight varies depending on the temperature history during polymerization, and imidization is carried out by heat, so it may not be possible to stably manufacture a polyimide precursor.

[0203] The obtained polyimide precursor (polyamic acid silyl ester) can be reacted in the same manner as the item 1) of polyamic acid (refer to the one-stage supply method, i.e., the second stage in which the temperature is low in the first stage-the temperature is high in the second stage and the temperature is low in the first stage-the temperature is low in the second stage). That is, in a certain embodiment, heating at a relatively high temperature, for example, 80°C or more, preferably 90°C or more, and more preferably 100°C or more, for example, for 5 minutes to 72 hours, can achieve the target imidization rate while suppressing excessive imidization reaction. In addition, in another embodiment, imidization can also be carried out at a relatively low temperature, for example, 0°C or more and 80°C or less (or less than 80°C), preferably 70°C or less, for a specified time, for example, 1 day to 1 year, to adjust the imidization rate.

[0204] 4) Polyamic acid silyl ester (direct method)

[0205] The polyamic acid solution having a predetermined imidization ratio obtained in the method 1) is mixed with a silylating agent and stirred at 0 to 120° C., preferably 5 to 80° C. for 1 to 72 hours to obtain polyamic acid silyl ester having a predetermined imidization ratio.

[0206] Alternatively, under conditions that tetracarboxylic dianhydride as a tetracarboxylic acid component and a diamine component are inhibited from imidizing, for example, they are reacted at a temperature of less than 100° C. to obtain a polyamic acid with a low imidization rate (refer to the first step when the heating stage is divided into two steps in the one-stage supply method of the item 1) polyamic acid above. ). A silylating agent is mixed in the obtained polyamic acid solution, and stirred at a temperature of 0 to 120° C., preferably 5 to 80° C. for 1 to 72 hours to obtain a polyamic acid silyl ester with a low imidization rate. The obtained polyimide precursor (polyamic acid silyl ester) is reacted in the same manner as the above 3) polyamic acid silyl ester (indirect method) to achieve the target imidization rate.

[0207] As the silylating agent used in the method 3) and the method 4), when a silylating agent that does not contain chlorine is used, it is not necessary to purify the silylated polyamic acid or the obtained polyimide, so it is preferred. As the silylating agent that does not contain chlorine atoms, N, O-bis (trimethylsilyl) trifluoroacetamide, N, O-bis (trimethylsilyl) acetamide, and hexamethyldisilazane can be cited. Because it does not contain fluorine atoms and has low cost, N, O-bis (trimethylsilyl) acetamide and hexamethyldisilazane are particularly preferred.

[0208] In the silylation reaction of diamine in the method 3), an amine catalyst such as pyridine, piperidine, triethylamine, etc. may be used to promote the reaction. The catalyst may be used directly as a polymerization catalyst for the polyimide precursor.

[0209] The solvent used in preparing the polyimide precursor is preferably water, or a non-protonic solvent such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, dimethyl sulfoxide, etc. Any type of solvent can be used without problem as long as it can dissolve the raw monomer components and the generated polyimide precursor, so there is no particular limitation on its structure. As the solvent, it is preferred to use water, or amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and N-ethyl-2-pyrrolidone, cyclic ester solvents such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, and α-methyl-γ-butyrolactone, carbonate solvents such as ethylene carbonate and propylene carbonate, glycol solvents such as triethylene glycol, phenol solvents such as m-cresol, p-cresol, 3-chlorophenol, and 4-chlorophenol, acetophenone, 1,3-dimethyl-2-imidazolidinone, cyclopentane, dimethyl sulfoxide, and the like. In addition, other common organic solvents may be used, i.e., phenol, o-cresol, butyl acetate, ethyl acetate, isobutyl acetate, propylene glycol methyl acetate, ethyl cellosolve, butyl cellosolve, 2-methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, tetrahydrofuran, dimethoxyethane, diethoxyethane, dibutyl ether, diethylene glycol dimethyl ether, methyl isobutyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, acetone, butanol, ethanol, xylene, toluene, chlorobenzene, turpentine, mineral spirits, naphtha-based solvents, etc. It should be noted that two or more solvents may be used in combination.

[0210] In the production of the polyimide precursor, there are no particular restrictions, and a monomer and a solvent are added so that the solid content concentration of the polyimide precursor (polyimide-converted mass concentration) is, for example, 5 to 45% by mass to carry out the reaction.

[0211] The logarithmic viscosity of the polyimide precursor is not particularly limited, but preferably the logarithmic viscosity in a 0.5 g / dL N,N-dimethylacetamide solution at 30° C. is 0.2 dL / g or more, more preferably 0.3 dL / g or more, and particularly preferably 0.4 dL / g or more. When the logarithmic viscosity is 0.2 dL / g or more, the molecular weight of the polyimide precursor is high, and the obtained polyimide has excellent mechanical strength and heat resistance.

[0212] <Preferred additives>

[0213] The polyimide precursor composition may contain an imidazole compound. The addition of an imidazole compound sometimes has an effect on improving the transmittance and / or reducing the linear thermal expansion coefficient, but depending on the selection of the compound, the imidization rate is sometimes easily increased. Therefore, when adding an imidazole compound, it is preferred to appropriately select the compound and / or appropriately adjust the imidization rate.

[0214] The imidazole compound is not particularly limited, and examples thereof include 1,2-dimethylimidazole, 1-methylimidazole, 2-methylimidazole, 2-phenylimidazole, imidazole, benzimidazole, etc. For the sake of stability of the polyimide precursor composition, it is preferred to use at least one imidazole compound selected from 2-phenylimidazole and benzimidazole.

[0215] The content of the imidazole compound in the polyimide precursor composition can be appropriately selected considering the balance between the addition effect and the stability of the polyimide precursor composition. The amount of the imidazole compound is preferably more than 0.01 mole and less than 1 mole relative to 1 mole of the repeating unit of the polyimide precursor. By adding the imidazole compound, mechanical properties such as elongation at break are usually improved. On the other hand, if the content of the imidazole compound is too much, the storage stability of the polyimide precursor composition sometimes deteriorates.

[0216] The content of the imidazole compound relative to 1 mol of the repeating unit is more preferably 0.02 mol or more, further more preferably 0.025 mol or more, further more preferably 0.05 mol or more, and more preferably 0.8 mol or less, further more preferably 0.6 mol or less, further more preferably 0.4 mol or less, further more preferably less than 0.4 mol, and most preferably 0.3 mol or less.

[0217] It should be noted that, in patent document 6 (International Publication No. 2015 / 080158), a polyimide precursor composition containing an imidazole compound is described, but the excellent storage stability of the polyimide precursor composition containing 2-phenylimidazole and / or benzimidazole is not disclosed. In addition, the embodiment of the document shows that the 400nm transmittance of the polyimide film manufactured from a composition containing 2-phenylimidazole or benzimidazole is reduced compared with 1,2-dimethylimidazole, 1-methylimidazole and 2-methylimidazole. On the other hand, the transparency of the polyimide film manufactured by combining a composition of 2-phenylimidazole and / or benzimidazole in the preferred polyimide precursor of the present invention (70 mol% or more of X1 comes from CpODA, 70 mol% or more of Y1 comes from DABAN) is improved, and contrary to the disclosure of patent document 6, a 400nm transmittance equal to or higher than that of 2-methylimidazole is obtained. Furthermore, it was confirmed that 2-phenylimidazole and benzimidazole were more effective in reducing the linear expansion coefficient than other imidazoles.

[0218] <Mixing of Polyimide Precursor Composition>

[0219] The polyimide precursor composition used in the present invention comprises at least one polyimide precursor and a solvent, and may further optionally comprise at least one imidazole compound as described above.

[0220] As a solvent, the above-mentioned solvent described as a solvent used in preparing a polyimide precursor can be used. Usually, the solvent used in preparing a polyimide precursor can be used directly, that is, in the state of a polyimide precursor solution, but it can also be diluted or concentrated and used as needed. The imidazole compound is dissolved and present in the polyimide precursor composition. There is no particular limitation on the concentration of the polyimide precursor, and it is usually 5 to 45% by mass in terms of polyimide conversion mass concentration (solid content concentration). Here, the polyimide conversion mass refers to the mass when all repeating units are completely imidized.

[0221] The viscosity (rotational viscosity) of the polyimide precursor of the present invention is not particularly limited, and is measured using an E-type rotational viscometer at a temperature of 25° C. and a shear rate of 20 sec. -1 The rotational viscosity measured under the conditions of is preferably 0.01 to 1000 Pa·sec, more preferably 0.1 to 100 Pa·sec. In addition, thixotropy can be imparted as required. In the above-mentioned range of viscosity, it is easy to handle during coating or film formation, and shrinkage cavities are suppressed and leveling properties are excellent, so a good coating can be obtained.

[0222] The polyimide precursor composition of the present invention may contain antioxidants, ultraviolet absorbers, fillers (inorganic particles such as silica, etc.), dyes, pigments, coupling agents such as silane coupling agents, primers, flame retardants, defoamers, leveling agents, rheology control agents (flow aids), etc. as needed. The polyimide precursor composition of the present invention preferably does not contain a chemical imidizing agent.

[0223] In addition, according to the research of the present inventors, it has been confirmed that when a polyimide precursor composition to which a specific siloxane compound is added is used, the warpage of the produced polyimide film / glass substrate laminate is reduced. In the present invention, a siloxane compound of a type that does not impair transparency may be added to the polyimide precursor composition in an appropriate amount, or the siloxane compound may not be contained at all.

[0224] The polyimide precursor composition can be prepared by adding an imidazole compound or a solution of an imidazole compound to the polyimide precursor solution obtained by the above method and mixing. The tetracarboxylic acid component and the diamine component may be reacted in the presence of an imidazole compound.

[0225] <<Application and film properties of polyimide precursor composition>>

[0226] By further promoting the imidization of the polyimide precursor of the present invention, polyimide can be manufactured. In the present invention, it is not particularly limited, and the known imidization method can be appropriately applied. The form of the obtained polyimide can preferably include a film, a laminate of a polyimide film and other substrates, a coating film, a powder, a bead, a molded body, a foam, etc.

[0227] Depending on the application, the thickness of the polyimide film is preferably 1 μm or more, more preferably 2 μm or more, further preferably 5 μm or more, for example 250 μm or less, preferably 150 μm or less, more preferably 100 μm or less, and further preferably 50 μm or less.

[0228] In one embodiment of the present invention, when measured with a film having a thickness of 10 μm, the 400 nm light transmittance of the polyimide film is preferably 79% or more, more preferably 80% or more. In addition, when measured with a film having a thickness of 10 μm, the yellowness (YI) of the polyimide film is preferably 3.2 or less, more preferably 3.0 or less, and most preferably 2.7 or less.

[0229] The polyimide film of the present invention has an extremely low linear thermal expansion coefficient. In one embodiment of the present invention, when measured with a film thickness of 10 μm, the linear thermal expansion coefficient (CTE) of the polyimide film from 150°C to 250°C is preferably 20 ppm / K or less, more preferably less than 20 ppm, and most preferably 15 ppm / K or less.

[0230] The polyimide film of the present invention has extremely high heat resistance. In one embodiment of the present invention, the 5% weight loss temperature of the polyimide is preferably 500°C or more, more preferably 505°C or more, and even more preferably 510°C or more. In the case of forming a gas barrier film on the polyimide by forming a transistor on the polyimide, if the heat resistance is low, expansion may sometimes occur between the polyimide and the barrier film due to outgassing accompanying the decomposition of the polyimide. Generally, high heat resistance is preferred, but depending on the application, properties other than heat resistance may also be required, and the 5% weight loss temperature may be 500°C or less.

[0231] Furthermore, in one embodiment of the present invention, the elongation at break of the polyimide film having a thickness of 10 μm is preferably 10% or more.

[0232] In another preferred embodiment of the present invention, the breaking strength of the polyimide film is preferably 150 MPa or more, more preferably 170 MPa or more, further preferably 180 MPa or more, further preferably 200 MPa or more, further preferably 210 MPa or more. The breaking strength can be, for example, a value obtained for a film having a thickness of about 5 to 100 μm.

[0233] It is particularly preferable that the above-mentioned preferred properties regarding the polyimide film are satisfied simultaneously.

[0234] The polyimide film can be manufactured using a known method. A representative method is the following method: a polyimide precursor composition is cast onto a substrate, and then, the substrate is heated and imidized to obtain a polyimide film. This method is described below in association with the manufacture of a polyimide film / substrate laminate. In addition, the polyimide precursor composition can also be cast onto a substrate, heated and dried, and after manufacturing a self-supporting film, the self-supporting film is peeled off from the substrate, for example, the film is held with a tenter, and heated and imidized in a state where it can be degassed from both sides of the film to obtain a polyimide film.

[0235] <<Manufacturing of polyimide film / substrate laminate and flexible electronic device>>

[0236] The polyimide film / substrate laminate of the present invention can be produced by the following steps: (a) a step of applying a polyimide precursor composition to a substrate; (b) heat-treating the polyimide precursor on the substrate to produce a laminate having a polyimide film laminated on the substrate (polyimide film / substrate laminate). The method for producing a flexible electronic device of the present invention uses the polyimide film / substrate laminate produced by the above steps (a) and (b), and further comprises the following steps: (c) a step of forming at least one layer selected from a conductor layer and a semiconductor layer on the polyimide film of the laminate; and (d) a step of peeling off the substrate and the polyimide film.

[0237] The polyimide precursor composition that can be used in the method of the present invention contains a polyimide precursor and a solvent. The polyimide precursor can use the substances described in the item of the polyimide precursor composition. The polyimide precursor described as a preferred substance in the item of the polyimide precursor composition is also preferred in the method of the present invention, and is not particularly limited.

[0238] First, in step (a), a polyimide precursor composition is cast on a substrate, and imidization and solvent removal are performed by heat treatment to form a polyimide film, thereby obtaining a laminate of the substrate and the polyimide film (polyimide film / substrate laminate).

[0239] As the substrate, a heat-resistant material is used, for example, a plate-like or sheet-like substrate of a ceramic material (glass, alumina, etc.), a metal material (iron, stainless steel, copper, aluminum, etc.), a semiconductor material (silicon, compound semiconductor, etc.), or a film or sheet-like substrate of a heat-resistant plastic material (polyimide, etc.). Generally, a flat and smooth plate is preferred, and generally, a glass substrate of soda-lime glass, borosilicate glass, alkali-free glass, sapphire glass, etc.; a semiconductor substrate (including compound semiconductor) of silicon, GaAs, InP, GaN, etc.; a metal substrate of iron, stainless steel, copper, aluminum, etc. is used.

[0240] Glass substrates are particularly preferred in the present invention. Flat, smooth, and large-area glass substrates have been developed and can be easily obtained. In particular, as the area of ​​the substrate increases, the problem of warping becomes significant. From the perspective of rigidity, the glass substrate is also more susceptible to warping. Therefore, the problem of using a glass substrate can be solved by applying the present invention. There is no limitation on the thickness of a plate-like substrate such as a glass substrate. From the perspective of ease of handling, it is, for example, 20 μm to 4 mm, preferably 100 μm to 2 mm. In addition, there is no particular limitation on the size of the plate-like substrate. One side (the long side in the case of a rectangle) is, for example, about 100 mm to about 4000 mm, preferably about 200 mm to about 3000 mm, and more preferably about 300 mm to about 2500 mm.

[0241] These glass substrates and other base materials may have an inorganic thin film (eg, a silicon oxide film) or a resin thin film formed on the surface.

[0242] The method for casting the polyimide precursor composition on the substrate is not particularly limited, and examples thereof include slit coating, die coating, blade coating, spray coating, inkjet coating, nozzle coating, spin coating, screen printing, rod coating, electrodeposition and the like.

[0243] In step (b), the polyimide precursor composition is heat-treated on the substrate to convert it into a polyimide film to obtain a polyimide film / substrate laminate. The heat treatment conditions are not particularly limited, and it is preferably dried in a temperature range of 50°C to 150°C, and then treated at a maximum heating temperature of, for example, 150°C to 600°C, preferably 200°C to 550°C, and more preferably 250°C to 500°C. The heat treatment conditions when using a polyimide solution are not particularly limited, and the maximum heating temperature is, for example, 100°C to 600°C, preferably 150°C or more, more preferably 200°C or more, and preferably 500°C or less, more preferably 450°C or less.

[0244] The thickness of the polyimide film is preferably 1 μm or more, more preferably 2 μm or more, and further preferably 5 μm or more. When the thickness is less than 1 μm, the polyimide film cannot maintain sufficient mechanical strength. For example, when used as a substrate for a flexible electronic device, it is sometimes unable to fully withstand stress and is damaged. In addition, the thickness of the polyimide film is preferably 100 μm or less, more preferably 50 μm or less, and further preferably 20 μm or less. If the thickness of the polyimide film becomes thicker, it sometimes becomes difficult to thin the flexible device. In order to maintain sufficient tolerance as a flexible device and further thin the film, the thickness of the polyimide film is preferably 2 to 50 μm.

[0245] Furthermore, in one embodiment of the present invention, the elongation at break of the polyimide film having a thickness of 10 μm is preferably 10% or more.

[0246] In another preferred embodiment of the present invention, the breaking strength of the polyimide film is preferably 150 MPa or more, more preferably 170 MPa or more, further preferably 180 MPa or more, further preferably 200 MPa or more, further preferably 210 MPa or more. The breaking strength can be, for example, a value obtained for a film having a thickness of about 5 to 100 μm.

[0247] It is particularly preferable that the above-mentioned preferred properties concerning the polyimide film and the laminate are satisfied simultaneously.

[0248] The polyimide film in the polyimide film / substrate laminate may also have a second layer such as a resin film or an inorganic film on the surface. That is, after forming the polyimide film on the substrate, the second layer may be laminated to form a flexible electronic device substrate. It is preferred to have at least an inorganic film, and it is particularly preferred to function as a barrier layer for water vapor or oxygen (air). As the water vapor barrier layer, for example, a material selected from silicon nitride (SiN x ), silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2) and other metal oxides, metal nitrides and metal oxynitrides. Generally, as the film forming methods of these thin films, physical vapor deposition methods such as vacuum evaporation, sputtering, and ion plating, and chemical vapor deposition methods (chemical vapor deposition methods) such as plasma CVD and catalytic chemical vapor deposition (Cat-CVD) are known. The second layer can also be a plurality of layers.

[0249] When the second layer is a plurality of layers, a resin film and an inorganic film may be composited. For example, a three-layer structure of barrier layer / polyimide layer / barrier layer may be formed on a polyimide film in a polyimide film / substrate laminate.

[0250] In step (c), at least one layer selected from a conductor layer and a semiconductor layer is formed on the polyimide film (including the case where a second layer such as an inorganic film is laminated on the surface of the polyimide film) using the polyimide / substrate laminate obtained in step (b). These layers may be formed directly on the polyimide film (including the case where the second layer is laminated), or may be formed indirectly after laminating other layers required for the device.

[0251] The conductor layer and / or semiconductor layer are selected appropriately according to the elements and circuits required by the target electronic device. In step (c) of the present invention, when at least one of the conductor layer and the semiconductor layer is formed, it is also preferred to form at least one of the conductor layer and the semiconductor layer on a polyimide film formed with an inorganic film.

[0252] The conductor layer and the semiconductor layer include both the case where they are formed on the entire surface of the polyimide film and the case where they are formed on a portion of the polyimide film. The present invention can be transferred to step (d) immediately after step (c), or after forming at least one layer selected from the conductor layer and the semiconductor layer in step (c), further forming a device structure, and then transferring to step (d).

[0253] In the case of manufacturing a TFT liquid crystal display device as a flexible device, for example, metal wiring, TFT using amorphous silicon or polycrystalline silicon, and transparent pixel electrodes are formed on a polyimide film having an inorganic film formed on the entire surface as required. The TFT includes, for example, a semiconductor layer such as a gate metal layer, an amorphous silicon film, a gate insulating layer, wiring connected to the pixel electrode, etc. In addition, the structure required for the liquid crystal display can be further formed by a known method. In addition, a transparent electrode and a color filter can also be formed on the polyimide film.

[0254] When manufacturing an organic EL display, for example, TFTs may be formed as needed on a polyimide film having an inorganic film formed on the entire surface in addition to transparent electrodes, a light-emitting layer, a hole transport layer, an electron transport layer, etc.

[0255] The polyimide film preferred in the present invention is excellent in various properties such as heat resistance and toughness, and therefore the method of forming circuits, elements, and other structures required for the device is not particularly limited.

[0256] Next, in step (d), the substrate and the polyimide film are peeled off. The peeling method may be a mechanical peeling method in which external force is applied to physically peel the film, or a so-called laser peeling method in which laser light is irradiated from the substrate surface to peel the film.

[0257] The structure or components required for the device are further formed or assembled on the (semi-)product using the polyimide film after the substrate is peeled off as a substrate to complete the device.

[0258] Example

[0259] The present invention is further described below by way of examples and comparative examples. It should be noted that the present invention is not limited to the following examples.

[0260] In the following examples, evaluation was performed by the following method.

[0261] <Evaluation of Polyimide Precursor Solution (Varnish)>

[0262] [Imidization rate]

[0263] The polyimide precursor solution was prepared by using dimethyl sulfoxide-d6 as solvent and M-AL400 manufactured by JEOL Ltd. 1 The imidization ratio [the content of the repeating unit represented by the chemical formula (2) relative to all repeating units] was calculated from the ratio of the integrated value of the peak of the aromatic proton to the integrated value of the peak of the carboxylic acid proton by the following formula (I) in the H-NMR measurement.

[0264] Imidization rate (%) = {X-(Y / Z)×A} / 2×100(I)

[0265] X: Integrated value of the amide proton peak when the imidization rate is 0% obtained from the amount of monomer charged

[0266] Y: By 1 The integral value of the amide proton peak obtained by H-NMR measurement

[0267] Z: By 1 The integral value of the aromatic proton peak obtained by H-NMR measurement

[0268] A: The integral value of the aromatic proton peak calculated from the amount of monomer charged

[0269] <Evaluation of polyimide film>

[0270] [400nm transmittance]

[0271] The light transmittance at 400 nm of a polyimide film having a film thickness of about 10 μm was measured using an ultraviolet-visible spectrophotometer / V-650DS (manufactured by JASCO Corporation).

[0272] [Yellowness (YI)]

[0273] The YI of the polyimide film was measured using a UV-visible spectrophotometer / V-650DS (manufactured by JASCO Corporation) in accordance with the standard of ASTEM E313. The light source was D65 and the viewing angle was 2°.

[0274] [Elastic modulus, elongation at break, breaking strength]

[0275] A polyimide film with a thickness of about 10 μm was punched into a dumbbell shape according to the IEC450 standard to prepare a test piece. The initial elastic modulus, elongation at break and breaking strength were measured using TENSILON manufactured by ORIENTEC at a chuck length of 30 mm and a tensile speed of 2 mm / min.

[0276] [Coefficient of linear thermal expansion (CTE)]

[0277] A polyimide film with a film thickness of about 10 μm was cut into strips with a width of 4 mm to prepare test pieces, and the temperature was raised to 500° C. using TMA / SS6100 (manufactured by SII Nanotechnology Co., Ltd.) under the conditions of a chuck spacing of 15 mm, a load of 2 g, and a heating rate of 20° C. / min. The linear thermal expansion coefficient from 150° C. to 250° C. was obtained from the obtained TMA curve.

[0278] [5% weight loss temperature]

[0279] A polyimide film having a thickness of about 10 μm was used as a test piece and heated from 25° C. to 600° C. at a heating rate of 10° C. / min in a nitrogen stream using a calorimeter measuring apparatus (Q5000IR) manufactured by TA INSTRUMENTS. The 5% weight loss temperature was determined from the obtained weight curve.

[0280] <Raw materials>

[0281] The abbreviations, purity, etc. of the raw materials used in the following examples are as follows.

[0282] [Diamine component]

[0283] DABAN: 4,4'-diaminobenzanilide

[0284] PPD: p-phenylenediamine

[0285] BAPB: 4,4'-bis(4-aminophenoxy)biphenyl

[0286] TPE-Q: 1,4-bis(4-aminophenoxy)benzene

[0287] TFMB: 2,2'-bis(trifluoromethyl)benzidine

[0288] [Tetracarboxylic acid component]

[0289] CpODA: Norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride

[0290] DNDAxx: (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethylnaphthalene-2t,3t,6c,7c-tetracarboxylic dianhydride

[0291] PMDA-H: Cyclohexanetetracarboxylic dianhydride

[0292] CBDA: Cyclobutanetetracarboxylic dianhydride

[0293] [Imidazole compounds]

[0294] 2-Pz: 2-phenylimidazole

[0295] Bz: benzimidazole

[0296] 2-Mz: 2-methylimidazole

[0297] [Solvent]

[0298] NMP: N-methyl-2-pyrrolidone

[0299] DMAc: dimethylacetamide

[0300] Table 1-1 shows the tetracarboxylic acid component and the diamine component used in Examples and Comparative Examples, and Table 1-2 shows the structural formula of the imidazole compound used in Examples and Comparative Examples.

[0301] [Table 1-1]

[0302]

[0303] [Table 1-2]

[0304]

[0305] <Example 1>

[0306] [Preparation of polyimide precursor composition]

[0307] 2.27 g (0.010 mol) of DABAN was added to a nitrogen-purged reaction container, and 32.11 g of N-methyl-2-pyrrolidone was added in an amount of 16% by mass of the total mass of the monomers (the sum of the diamine component and the carboxylic acid component), and stirred at 50° C. for 1 hour. 3.84 g (0.010 mol) of CpODA was slowly added to the solution. Stirring was performed at 70° C. for 4 hours to obtain a uniform and viscous polyimide precursor solution.

[0308] 2-phenylimidazole as an imidazole compound was dissolved in 4 times the mass of N-methyl-2-pyrrolidone to obtain a uniform solution with a solid content concentration of 20% by mass of 2-phenylimidazole. The solution of the imidazole compound was mixed with the above-synthesized polyimide precursor solution in such a manner that the amount of the imidazole compound was 0.025 moles per 1 mole of the repeating unit of the polyimide precursor, and stirred at room temperature for 3 hours to obtain a uniform and viscous polyimide precursor composition. The imidization rate of the polyimide precursor in the obtained polyimide precursor composition was measured and the result was 18%.

[0309] [Manufacturing of polyimide film]

[0310] As a glass substrate, a 6-inch Eagle-XG (registered trademark) manufactured by Corning Incorporated (500 μm thick) was used. The polyimide precursor composition was applied to the glass substrate using a spin coater, and the glass substrate was directly heated from room temperature to 415°C under a nitrogen atmosphere (oxygen concentration of less than 200 ppm), and imidization was performed thermally to obtain a polyimide film / substrate laminate. The laminate was immersed in water at 40°C (e.g., a temperature range of 20°C to 100°C), the polyimide film was peeled off from the glass substrate, and after drying, the properties of the polyimide film were evaluated. The film thickness of the polyimide film was about 10 μm. The evaluation results are shown in Table 2.

[0311] <Examples 2 to 10>

[0312] In Example 1, the imidazole compound was changed to the compound shown in Table 2 (blank column indicates no addition), and a polyimide precursor composition containing a polyimide precursor having an imidization rate shown in Table 2 was obtained in the same manner as in Example 1. Thereafter, a polyimide film was produced in the same manner as in Example 1, and the film properties were evaluated. The results are shown in Table 2. It should be noted that among Examples 1 to 10, the long-term stability of the polyimide precursor compositions of Examples 1 to 5 and 8 to 10 was also very excellent. All physical properties of Examples 1 to 5 were excellent.

[0313] <Examples 11 to 17, Comparative Examples 1 to 3>

[0314] In Example 1, the imidazole compound was changed to the compound shown in Table 3. In addition, in Example 1, the temperature and time after adding CpODA were changed to obtain a polyimide precursor composition containing a polyimide precursor having an imidization rate shown in Table 3. Thereafter, a polyimide film was produced in the same manner as in Example 1, and the film properties were evaluated. The results are shown in Table 3.

[0315] <Examples 18 to 22, Comparative Example 4>

[0316] In Example 1, the diamine component and the imidazole compound were changed to the compounds shown in Table 4. In addition, the temperature and time after adding CpODA were changed in Example 1, thereby obtaining a polyimide precursor composition containing a polyimide precursor having an imidization rate shown in Table 4. Thereafter, a polyimide film was produced in the same manner as in Example 1, and the film properties were evaluated. The results are shown in Table 4.

[0317] <Examples 23 to 29, Comparative Examples 5 and 6>

[0318] In Example 1, the tetracarboxylic acid component, the diamine component and the imidazole compound were changed to the compounds shown in Table 5. In addition, the temperature and time after adding CpODA were changed in Example 1, thereby obtaining a polyimide precursor composition containing a polyimide precursor having an imidization rate shown in Table 5. Thereafter, a polyimide film was produced in the same manner as in Example 1, and the film properties were evaluated. The results are shown in Table 5.

[0319] <Comparative Examples 7 to 10>

[0320] In Example 1, the tetracarboxylic acid component, the diamine component and the imidazole compound were changed to the compounds shown in Table 6. In addition, the temperature and time after adding CpODA were changed in Example 1, thereby obtaining a polyimide precursor composition containing a polyimide precursor having an imidization rate shown in Table 6. Thereafter, a polyimide film was produced in the same manner as in Example 1, and the film properties were evaluated. The results are shown in Table 6.

[0321] <Comparative Example 11>

[0322] In a nitrogen-substituted reaction vessel, 0.713 g (3.136 mmol) of DABAN and 1.004 g (3.136 mmol) of TFMB were added, and 16.5 g of DMAc was added to reach 20% by mass of the total mass of the monomers (the sum of the diamine component and the carboxylic acid component), and the mixture was stirred at room temperature for 1 hour. 2.411 g (6.272 mmol) of CpODA was slowly added to the solution, and the mixture was stirred at room temperature for 24 hours. After that, the temperature was raised to 160°C, 25 mL of toluene was added, and after the toluene was refluxed for 10 minutes, the toluene was extracted and cooled to room temperature to obtain a uniform and viscous polyimide precursor solution (imidization rate: 44%). After that, a polyimide film was manufactured in the same manner as in Example 1, and the film properties were evaluated. The results are shown in Table 6.

[0323] [Table 2]

[0324]

[0325] [Table 3]

[0326]

[0327] [Table 4]

[0328]

[0329] [Table 5]

[0330]

[0331] [Table 6]

[0332]

[0333] From the above results, it can be seen that the polyimide film obtained from the polyimide precursor composition in which the proportion of CpODA in the tetracarboxylic acid component is 70 mol% or more, the proportion of DABAN in the diamine component is 70 mol% or more, and the imidization rate is less than 50% has a large 400nm transmittance, a small linear thermal expansion coefficient, and a high 5% weight loss temperature.

[0334] Industrial Applicability

[0335] The present invention can be suitably used in the manufacture of flexible electronic devices, such as display devices such as liquid crystal displays, organic EL displays and electronic paper, and light receiving devices such as solar cells and CMOS.

Claims

1. A polyimide precursor composition, It is characterized in that It contains: A polyimide precursor, wherein the repeating unit is composed of a repeating unit represented by the following general formula (I) and a repeating unit of the general formula (I) that is further imidized, and the imidization rate is 12% or more and less than 50%; and Solvents, [Chemistry 1] In the general formula I, X 1 is a tetravalent aliphatic group or an aromatic group, Y 1 is a divalent aliphatic group or an aromatic group, R 1 and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms, wherein X 1 70 mol% or more of the structure represented by formula (1-1), [Chemistry 2] Y 1 70 mol% or more of the structure represented by formula (D-1) and / or (D-2) [Chemistry 3] 2. The polyimide precursor composition according to claim 1, It is characterized in that The polyimide film obtained from the polyimide precursor composition has a light transmittance of 79% or more at a wavelength of 400 nm in the case of a film having a thickness of 10 μm.

3. The polyimide precursor composition according to claim 1, It is characterized in that The polyimide film obtained from the polyimide precursor composition has a linear thermal expansion coefficient of 20 ppm / K or less at 150° C. to 250° C. in the case of a film having a thickness of 10 μm.

4. The polyimide precursor composition according to claim 1, It is characterized in that The polyimide obtained from the polyimide precursor composition has a 5% weight loss temperature of 500° C. or higher.

5. The polyimide precursor composition according to claim 1, It is characterized in that The polyimide film obtained from the polyimide precursor composition has a breaking elongation of 10% or more in the case of a film having a thickness of 10 μm.

6. The polyimide precursor composition according to claim 1, It is characterized in that X 1 90 mol % or more of the above structure is represented by the formula (1-1). 7 . A polyimide film obtained from the polyimide precursor composition according to claim 1 .

8. A polyimide film / substrate laminate, It is characterized in that It has: A polyimide film obtained from the polyimide precursor composition according to any one of claims 1 to 6; and Base material.

9. The laminate according to claim 8, in, The substrate is a glass substrate.

10. A method for producing a polyimide film / substrate laminate, comprising: (a) a step of applying the polyimide precursor composition according to any one of claims 1 to 6 onto a substrate; and (b) A step of heat-treating the polyimide precursor on the substrate to laminate a polyimide film on the substrate.

11. The manufacturing method according to claim 10, in, The substrate is a glass substrate.

12. A method for manufacturing a flexible electronic device, comprising: (a) a step of applying the polyimide precursor composition according to any one of claims 1 to 6 onto a substrate; (b) a step of heat-treating the polyimide precursor on the substrate to produce a polyimide film / substrate laminate in which a polyimide film is laminated on the substrate; (c) forming at least one layer selected from a conductor layer and a semiconductor layer on the polyimide film of the laminate; and (d) A step of peeling the substrate and the polyimide film.

13. The manufacturing method according to claim 12, in, The substrate is a glass substrate.

Citation Information

Patent Citations

  • Polyimide precursor resin composition for flexible device substrates and method for producing flexible device using the same, and flexible device

    JP2010202729A

  • Polyimide precursor, polyimide, and materials to be used in producing same

    WO2012011590A1

  • Polyimide precursor and polyimide

    WO2013179727A1

  • Polyimide precursor, polyimide, varnish, polyimide film, and substrate

    WO2014038715A1

  • Mixing spatula

    WO2014067079A1