A high wear-resistant steel plate and online manufacturing method thereof

By designing high-Si and Mn alloys and employing an online air-cooled hardening stacking self-tempering process, medium-carbon bainitic/martensitic multiphase steel plates were prepared. This solved the problem of bulk spalling of wear-resistant steel plates under special operating environments, and enabled the production of wear-resistant steel plates with high hardness, good toughness, and low cost.

CN116463549BActive Publication Date: 2024-11-29SD STEEL RIZHAO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310285690.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-11-29
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Existing wear-resistant steel plates are prone to spalling in large pieces under special operating environments, resulting in high production costs and problems such as high energy consumption and waste of alloy resources.

Method used

By employing a high Si and Mn alloying element design, combined with online air-cooling hardening and stacking self-tempering processes, a high wear-resistant steel plate with a medium-carbon bainitic/martensite dual-phase structure is prepared. The addition of precious elements Mo and Ni is omitted, and the microstructure is balanced by controlling the cooling rate and stacking temperature.

Benefits of technology

While maintaining ultra-high hardness, it significantly improves the toughness and impact resistance of steel plates, wear uniformity and anti-stripping properties, reduces production costs and energy consumption, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116463549B_ABST
    Figure CN116463549B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of wear-resistant steel preparation, and in particular to a high-wear-resistant steel plate and an online manufacturing method thereof. The chemical composition and weight percentage of the steel plate include C: 0.18%-0.35%, Si: 1.00%-1.50%, Mn: 1.80%-2.50%, P<0.010%, S<0.003%, Als: 0.015%-0.035%, Cr: 0.20%-0.40%, V: 0.020%-0.060%, and meets C+Mn / 10+Cr / 15+3V≤0.65%, and the rest is Fe and unavoidable impurities. The present invention reduces the carbon content, reasonably adjusts the relative contents of economic elements such as Si, Mn, Cr, V, and controls C+Mn / 10+Cr / 15+3V which has an important influence on wear resistance, omits the long process offline quenching and tempering process of traditional wear-resistant steel, and adopts an appropriate online air cooling short process to achieve the final balanced microstructure ratio. The obtained steel plate has ultra-high hardness, good toughness and plasticity, and excellent wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wear-resistant steel preparation technology, specifically to a high wear-resistant steel plate and its online manufacturing method. Background Art

[0002] Wear-resistant steel plates are mainly used in the construction machinery industry for wear-resistant working parts and structures of excavators, loaders, bulldozers, graders, large off-highway dump trucks, electric wheels, etc., as well as equipment parts in mining, ore dressing, docks, cement plants, and steel mills that require material transportation and are subject to wear and erosion. The consumption of wear-resistant steel is enormous. With increased national investment in public infrastructure such as highways and railways, energy construction, and water conservancy projects, the market demand for wear-resistant steel has grown rapidly. In the past, domestic wear-resistant steel was mainly made of high-carbon, high-manganese, high-chromium, and high-nickel materials, with the common process being quenching and tempering. This production method had problems such as insufficient environmental protection and energy conservation, and insufficient use of alloy resources. Especially in metallurgical mines, coal mining, and transportation, where there are massive amounts of material collapses, vibrations, and impacts, the special impact friction and sliding friction alter the wear mechanism of steel. Conventional wear-resistant steel exhibits a phenomenon of flaking off in chunks during use, commonly known as "losing flesh." Therefore, downstream users generally request that wear-resistant steel have both increased hardness and toughness reserves to ensure uniform wear of wear-resistant parts and improve service life.

[0003] The patent application "High-Toughness Ultra-High-Strength Wear-Resistant Steel Plate and Its Production Method" (application number: 200910013285.1) discloses a steel plate with the following chemical composition: C 0.15%~0.26%, Si 0.20%~0.55%, Mn 1.0%~1.60%, P≤0.020%, S≤0.010%, Mo0.00%~0.60%, Ni 0.00%~0.50%, Cr 0.20%~1.00%, Ti 0.01%~0.05%, Als 0.02%~0.04%, B0.0005%~0.004%, with the balance being Fe and unavoidable impurities. The technical solution adopts a heat treatment process of rolling followed by quenching and tempering to obtain a tempered martensitic structure; the composition is a conventional Mo, Ni, Cr, B system, and the hardness level is 420-480 HBW. This technical solution involves adding Mo and Ni to precipitate M. x C y Improving the strength and toughness of wear-resistant steel by using precious alloying elements such as wear-resistant particles inevitably increases production costs. Adding processes such as offline quenching and tempering heat treatment results in a tempered martensitic structure with high phase transformation stress and limited toughness reserves. It also contains significant residual stress, which can easily cause cracking at the plate-strip interface during use, eventually leading to blocky "meat loss." Furthermore, it requires specialized equipment, increases process costs, and faces practical problems such as high energy consumption.

[0004] Therefore, there is an urgent need to develop a long-life wear-resistant steel plate with balanced microstructure, ultra-high hardness, and good toughness and ductility, and its online short-process manufacturing method. Summary of the Invention

[0005] To address the technical problems of high production costs caused by adding expensive alloying elements such as Mo and Ni, large residual stress within the tempered martensite structure, and increased process costs, this invention provides a high wear-resistant steel plate and its online manufacturing method. It omits the addition of expensive elements Mo and Ni, instead employing inexpensive alloying elements Si and Mn. Through a post-rolling online air-cooling hardening + stacking self-tempering process, a high wear-resistant steel plate with a balanced medium-carbon bainite + martensite microstructure is obtained. This allows the steel plate to achieve ultra-high hardness while maintaining good toughness reserves. The resulting steel plate possesses excellent wear resistance and impact resistance, meeting the requirements of the special operating environments in metallurgical mining, coal mining, and transportation processes for uniform wear of working components and extended service life.

[0006] In a first aspect, the present invention provides an online manufacturing method for a high wear-resistant steel plate, wherein the chemical composition and weight percentage of the steel plate include C: 0.18%-0.35%, Si: 1.00%-1.50%, Mn: 1.80%-2.50%, P<0.010%, S<0.003%, Als: 0.015%-0.035%, Cr: 0.20%-0.40%, V: 0.020%-0.060%, and meets the condition that C+Mn / 10+Cr / 15+3V≤0.65%, with the remainder being Fe and unavoidable impurities;

[0007] Online manufacturing methods include at least the following steps:

[0008] a) Straightening of continuously cast billets, controlling the temperature of the straightening section above 900℃;

[0009] b) Steel billets are directly hot-delivered, with the hot-delivery temperature controlled at 150-400℃ or above 550℃;

[0010] c) Reheat the steel billet, controlling the reheating temperature at 1200-1250℃;

[0011] d) Rolling, controlling the final rolling temperature at 780-820℃;

[0012] e) After rolling, the steel plates are directly air-cooled to 350°C, and the steel plates are quickly removed from the production line and stacked. The temperature of the steel plates is controlled at 260-350°C during stacking, and hot steel plates are laid on the bottom and covered with a top cover.

[0013] Furthermore, in step d), the rolling speed at the high temperature stage above 950℃ is ≤1.2m / s, and the product is rolled into finished product using a forward rolling method.

[0014] Furthermore, in step d), the steel throwing speed in the final rolling pass is ≤2m / s.

[0015] Furthermore, in step e), samples are taken after stacking for 96 hours to test mechanical properties.

[0016] Secondly, the present invention provides a high wear-resistant steel plate prepared by the above-described online manufacturing method.

[0017] Furthermore, the microstructure of the high wear-resistant steel plate is a medium-carbon bainite / martensite dual phase, with a bainite volume fraction >40%.

[0018] Furthermore, the maximum thickness of the high wear-resistant steel plate is 60 mm.

[0019] Furthermore, the high wear-resistant steel plate has a yield strength of 1400-1650MPa, a tensile strength of 1600-2000MPa, an elongation of ≥14%, a low-temperature impact CVN (-40℃, transverse) of ≥30J, and a hardness of 500-570HBW; the relative wear resistance coefficient of the low alloy steel Q345B is ≥2.5.

[0020] This invention employs a high Si and Mn design, with the addition of economical elements such as Cr and V, and utilizes an online air-cooling short-process technology to achieve ultra-high hardness, uniform wear resistance, and long service life of 500-570 HBW wear-resistant steel. This meets the demands of high-stress and impact applications such as large dump trucks and electric wheel vehicles for uniform wear resistance and long service life. The main advantages are:

[0021] (1) Unique composition system, with both ultra-high hardness and good toughness and plasticity:

[0022] An economical high-Si, Mn, Cr alloying element design system is adopted, and the bainite transformation initiation temperature B is reduced by designing with high Mn content. S And it does not significantly reduce M S The main principle is to obtain refined medium-carbon bainite + martensite to improve the toughness and plasticity of steel plates. It fully utilizes the beneficial effects of Si in suppressing temper brittleness and improving temper resistance, as well as the principle that high Si promotes the distribution of carbon from martensite to retained austenite during the tempering process. This results in steel plates whose performance changes little over a wide range of stacking and self-tempering temperatures. While maintaining ultra-high hardness, they still have good plasticity and toughness indicators, meeting the user's demand for high-hardness steel with high toughness reserves.

[0023] (2) The process of air-cooled self-hardening and stacking self-tempering is simple, short, and has significant energy-saving and consumption-reducing effects:

[0024] The specially designed high-Si, Mn steel can obtain a bainite + martensite dual-phase structure under air cooling conditions, and can achieve self-tempering function by slow cooling in the low-temperature transformation zone below 350℃ through stacking. While achieving the final comprehensive performance, it eliminates the offline quenching + tempering process, which is in line with the current development trend of green, low-carbon and short-process production and manufacturing technology.

[0025] (3) The product has excellent uniform wear and anti-stripping properties:

[0026] By rationally controlling the relative contents of economical elements such as Si, Mn, Cr, and V, as well as the C+Mn / 10+Cr / 15+3V ratio which has a significant impact on wear resistance, and by leveraging the refined bainite in the steel and the high-carbon residual austenite distributed during the stacking self-tempering process, good plasticity and toughness indicators are obtained. The toughness and plasticity are improved by refining the grains through low-temperature final rolling, thereby ensuring uniform wear in actual working conditions of ultra-high hardness steel. Its anti-stripping (scraping) performance is more than 10 times that of other products, and its wear resistance is more than 2.5 times that of Q345 low alloy steel. Attached Figure Description

[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 This is a micrograph of the steel plate prepared in Example 1.

[0029] Figure 2 These are micrographs of the steel plate prepared in Example 2. Detailed Implementation

[0030] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.

[0031] Example 1

[0032] A high wear-resistant steel plate with a thickness of 60mm has the following chemical composition by weight percentage:

[0033] C 0.31%, Si 1.42%, Mn 2.38%, P 0.008%, S 0.001%, Als 0.017%, Cr 0.36%, V 0.023%, C+Mn / 10+Cr / 15+3V=0.64%, the remainder is Fe and unavoidable impurities.

[0034] The production methods for steel plates are as follows:

[0035] The raw materials undergo smelting, deoxidation and alloying, refining and continuous casting processes to obtain high-quality billets, and

[0036] a) The billet casting speed is coordinated with the cooling water, and the actual temperature of the straightening section of the continuously cast billet is calculated to be 915℃.

[0037] b) Steel billets are directly hot-delivered, with the hot-delivery temperature controlled at 380℃;

[0038] c) Reheat the steel billet, controlling the reheating temperature at 1230℃ and the heating time at 8min / cm;

[0039] d) Rolling: The rolling speed in the high-temperature stage above 950℃ is controlled at 1.15m / s, and the rolling is done in the direction of rolling. The final rolling temperature is controlled at 790℃, and the steel removal speed in the final rolling pass is 1.8m / s.

[0040] e) After rolling, the steel plates are quickly stacked off the roller conveyor. The temperature of the steel plates during stacking is 348℃. Other high-temperature hot-rolled steel plates are used as the bottom and top cover. After stacking for 96 hours, the stack is uncovered and sample plates are taken for testing.

[0041] The 60mm steel plate produced contains 48% bainite in its microstructure. Its mechanical properties are: yield strength 1480MPa, tensile strength 1650MPa, elongation 17%, average impact energy at -40℃ (transverse) reaches 46J, hardness 528HBW, and wear resistance tested by ring block wear test is 2.8 times that of Q345 low alloy steel.

[0042] Example 2

[0043] A high wear-resistant steel plate with a thickness of 22mm has the following chemical composition by weight percentage:

[0044] C 0.23%, Si 1.18%, Mn 1.93%, P 0.007%, S 0.002%, Als 0.029%, Cr 0.22%, V 0.051%, C+Mn / 10+Cr / 15+3V=0.59%, the remainder is Fe and unavoidable impurities.

[0045] The production methods for steel plates are as follows:

[0046] The raw materials undergo smelting, deoxidation and alloying, refining, and continuous casting processes to obtain high-quality cast billets, and

[0047] a) The billet casting speed and cooling water are coordinated, and the actual temperature of the straightening section of the continuously cast billet is calculated to be 907℃.

[0048] b) Steel billets are directly hot-delivered, with the hot-delivery temperature controlled at 620℃;

[0049] c) Reheat the billet, controlling the reheating temperature at 1210℃ and the heating time at 7min / cm;

[0050] d) Rolling: The rolling speed in the high-temperature stage above 950℃ is controlled at 1.08m / s, and the rolling is done in the direction of rolling. The final rolling temperature is controlled at 815℃, and the steel removal speed in the final rolling pass is 1.65m / s.

[0051] e) After rolling, the steel plates are quickly stacked off the roller conveyor. The temperature of the steel plates during stacking is 290℃. Other high-temperature hot-rolled steel plates are used as the bottom cover. After stacking for 96 hours, the stack is uncovered, and sample plates are taken for testing.

[0052] The 22mm steel plate produced contains 41% bainite in its microstructure. Its mechanical properties are: yield strength 1610MPa, tensile strength 1818MPa, elongation 15.5%, average impact energy at -40℃ (transverse) reaches 35J, hardness 562HBW, and wear resistance tested by ring block wear test is 3.1 times that of Q345 low alloy steel.

[0053] Although the present invention has been described in detail with reference to the accompanying drawings and preferred embodiments, the present invention is not limited thereto. Various equivalent modifications or substitutions can be made to the embodiments of the present invention by those skilled in the art without departing from the spirit and essence of the invention, and such modifications or substitutions should all be within the scope of the present invention. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should also be covered within the protection scope of the present invention.

Claims

1. An online manufacturing method for a high wear-resistant steel plate, characterized in that: The chemical composition and weight percentage of the steel plate include C: 0.18%-0.35%, Si: 1.00%-1.50%, Mn: 1.80%-2.50%, P<0.010%, S<0.003%, Als: 0.015%-0.035%, Cr: 0.20%-0.40%, V: 0.020%-0.060%, and meet C+Mn / 10+Cr / 15+3V≤0.65%, and the rest are Fe and unavoidable impurities; The online manufacturing method comprises at least the following steps: a) Straightening of continuous casting billets, controlling the temperature of the straightening section to be above 900°C; b) Direct hot delivery of billets, controlling the hot delivery temperature at 150-400℃, or above 550℃; c) Reheating of the steel billet, controlling the reheating temperature at 1200-1250℃; d) Rolling, controlling the final rolling temperature at 780-820℃; e) After rolling, the steel plates are directly air-cooled to 350°C, and the steel plates are quickly stacked off the production line. The temperature of the steel plates during stacking is controlled at 260-350°C, and hot steel plates are used for laying down and covering; The microstructure of high wear-resistant steel plate is medium carbon bainite / martensite duplex phase, and the volume fraction of bainite is >40%; The yield strength of high wear-resistant steel plate is 1400-1650MPa, the tensile strength is 1600-2000MPa, the elongation is ≥14%, the transverse Charpy impact energy at -40℃ is ≥30J, and the hardness is 500-570HBW; the relative wear resistance coefficient relative to low alloy steel Q345B is ≥2.

5.

2. The online manufacturing method according to claim 1, characterized in that: In step d), the rolling speed in the high temperature stage above 950° C. is ≤1.2 m / s, and the product is rolled in a forward rolling manner.

3. The online manufacturing method according to claim 1, characterized in that: In step d), the steel throwing speed in the final rolling pass is ≤2m / s.

4. The online manufacturing method according to claim 1, characterized in that: In step e), samples are taken after stacking for 96 hours to test the mechanical properties.

5. A high wear-resistant steel plate manufactured by the online manufacturing method according to claim 1.

6. The high wear-resistant steel plate according to claim 5, characterized in that: The maximum thickness of high wear resistant steel plate is 60mm.

Citation Information

Patent Citations

  • High-toughness and ultrahigh-strength wear-resistant steel plate and production method thereof

    CN101638755A

  • Abrasion-resistant steel sheet and method for producing abrasion-resistant steel sheet

    CN108884531A

  • Plastic mold steel plate and production method thereof