Preparation method of light-colored conductive nylon

Through solution fluid spinning method and laser heating technology, combined with spherical and needle-shaped blended fillers, the problem of difficult to balance the conductivity and mechanical properties of light-colored conductive fibers is solved, and the effects of high conductivity and high spinning rate are achieved.

CN116463747BActive Publication Date: 2024-11-26NANTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310464033.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-26
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

The conductivity and mechanical properties of existing light-colored conductive fibers are difficult to take into account during the melt spinning process. The high viscosity of the spinning liquid leads to random orientation of conductive whiskers, low drafting efficiency, and low heating efficiency of traditional heat rollers, which affects spinning. rate.

Method used

The solution fluid spinning method is used to disperse conductive filler with ultrasonic dispersion, and conducting nylon is formed through screw extrusion and multiple drafting. The laser heating is used to quickly heat up, combining spherical and needle-shaped blended filler to improve the conductivity and mechanical properties.

Benefits of technology

The improvement of conductive properties and the optimization of mechanical properties are achieved, and high conductivity is obtained through low addition amount, which solves the problems of large viscosity and low drafting efficiency of spinning fluid, and improves the stability of spinning rate and conductive properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a preparation method of light-colored conductive nylon, which adopts solution fluid spinning to replace traditional melt spinning. Since the solution fluid has a lower viscosity than the melt and has good fluidity, the rotational resistance of the conductive whisker in the spinning solution is also relatively small, and the orientation is easier to control, and there is no problem of sudden drop in fluidity after the spinning solution is ejected. Subsequently, the orientation degree of the conductive filler along the axial direction of the fiber is further improved by the drafting-inducing orientation method, and the axial conductivity of the charge is improved, so as to achieve high conductivity of the fiber with a lower addition amount. In the drafting system, a laser heating device is used to replace the traditional hot roller, and the temperature is quickly and accurately raised, the drafting effect is improved, and the spinning rate is increased. Fillers of different shapes have a great influence on the thermal conductivity and mechanical properties of the material. The conductive filler in the present invention is preferably spherical and needle-shaped blended, and the weight ratio of spherical and needle-shaped fillers is 1:0.5-2. A small amount of addition can obtain good electrical conductivity, which is conducive to the improvement of mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile processing, and particularly relates to a method for preparing light-colored conductive nylon. Background Art

[0002] The main means of realizing existing light-colored conductive fibers is to add titanium dioxide, potassium titanate, etc. that have been treated with conductive coating as light-colored conductive fillers during the melt spinning process. Among them, the use of spherical conductive fillers has little effect on the viscosity and fluidity of the spinning melt, and the spinning difficulty is small. Therefore, the existing technology mostly adds spherical fillers for melt spinning. However, when using spherical fillers to prepare conductive fibers, the percolation threshold of the fiber is high, and a high addition amount is required to achieve the ideal conductivity, resulting in the problem that the spinnability and mechanical properties of the fiber cannot be balanced with the conductive properties. Because whisker-like conductive fillers have a higher aspect ratio, when used, they are easier to form a conductive path through overlap than spherical fillers and are not easily damaged by fiber deformation. The conductive properties are better and more stable, and the higher the orientation degree of the filler, the better the conductive properties of the fiber. However, the addition of whisker-like fillers easily leads to excessive viscosity of the spinning melt, which is not conducive to high-multiple drafting, resulting in a low orientation degree of the filler along the fiber axis.

[0003] When light-colored conductive fibers are prepared by melt spinning, the orientation resistance of the conductive whiskers is large due to the high viscosity of the spinning solution. Therefore, the conductive whiskers in the obtained fibers are generally randomly oriented and have low axial charge conduction capacity. The multi-stage drawing method can induce the conductive whiskers to be oriented along the fiber axis to a certain extent through multiple drawing, thereby improving the conductivity of the fiber. However, due to the high viscosity of the spinning melt and the sudden drop in temperature after extrusion from the spinneret, the fluidity decreases, which is not conducive to drawing. In addition, the traditional hot roller heating efficiency used in multi-stage hot drawing is low, and the spinning rate is low. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing light-colored conductive nylon, comprising the following steps:

[0005] (1) Weigh a light-colored conductive filler, add it to a formic acid solution, and fully disperse it using an ultrasonic disperser in an ice bath;

[0006] (2) placing the uniformly dispersed formic acid suspension on a stirrer and rapidly stirring, while adding nylon chips into the suspension to obtain a spinning solution after the nylon chips are completely dissolved;

[0007] (3) The spinning solution is added to a screw extruder for extrusion, hot air is passed through the spinning tunnel, and high-multiple drawing is achieved through a rapidly rotating first drawing roller. During the drawing process, the solvent of the spinning solution is continuously evaporated, and the fiber is formed and wound on the first drawing roller. The fiber is then rapidly heated by a laser-assisted heating method and is drawn for a second time through a second drawing roller to obtain a light-colored conductive nylon.

[0008] The light-colored conductive filler in step (1) is at least one of conductive TiO2, conductive potassium titanate, etc. with a core-shell structure. The shell layer of the light-colored conductive filler is a conductive component, and its composition is at least one of antimony-doped tin oxide, tin-doped indium oxide, aluminum-doped zinc oxide, etc., and its shape is at least one of spherical, needle-shaped, etc., with a diameter within 250nm. Preferably, spherical and needle-shaped blended conductive fillers are used, and the weight ratio is 1:0.5-2.

[0009] The concentration of nylon in the spinning solution in step (2) is 25-35wt.%.

[0010] In step (3), the temperature of the first stretching roller is 40-60°C, and the stretching ratio is 8-15; the stretching ratio of the second stretching roller is 6-12, and the laser heating power is 1.2W.

[0011] The weight ratio of nylon to filler is 1:0.2-0.6.

[0012] The above technical scheme of the present invention has at least the following beneficial effects: The present invention provides a method for preparing light-colored conductive nylon, which adopts solution fluid spinning to replace traditional melt spinning. Since the solution fluid has a lower viscosity than the melt and has good fluidity, the rotational resistance of the conductive whiskers in the spinning solution is also relatively small, and the orientation is easier to control, and there is no problem of sudden drop in fluidity after the spinning solution is ejected. Subsequently, the orientation degree of the conductive filler along the axial direction of the fiber is further improved by the drafting-induced orientation method, and the axial conductivity of the charge is improved, so as to achieve high conductivity of the fiber with a lower addition amount. In the drafting system, a laser heating device is used to replace the traditional hot roller to quickly and accurately achieve rapid heating of the fiber, improve the drafting effect, and increase the spinning rate. Fillers of different shapes have a great influence on the thermal conductivity and mechanical properties of the material. The conductive filler in the present invention is preferably a spherical and needle-shaped blend, and the weight ratio of the spherical and needle-shaped fillers is 1:0.5-2. A small amount of addition can obtain good conductivity, which is conducive to the improvement of mechanical properties. DETAILED DESCRIPTION

[0013] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0014] Embodiment 1:

[0015] A method for preparing light-colored conductive nylon comprises the following steps:

[0016] 1) First weigh the light-colored conductive filler TiO 2 , added into the formic acid solution, and fully dispersed using an ultrasonic disperser, the dispersion process was carried out in an ice bath;

[0017] 2) placing the uniformly dispersed formic acid suspension on a stirrer and stirring rapidly, and at the same time adding nylon chips into the suspension to obtain a spinning solution after the nylon chips are completely dissolved;

[0018] 3) The spinning solution is added to the screw extruder and extruded, hot air is passed through the spinning tunnel, and high-multiple drawing is achieved through the rapidly rotating first drawing roller. The solvent of the spinning solution is continuously evaporated during the drawing process, and the fiber is formed and wound on the first drawing roller. The fiber is then quickly heated by a laser-assisted heating method and is drawn twice through a second drawing roller to obtain light-colored conductive nylon.

[0019] The conductive filler is in the shape of a mixture of spheres and needles, and the weight ratio of the needles to the spheres is 1:1.5.

[0020] The concentration of nylon in the spinning solution in step (2) is 25 wt.%.

[0021] The weight ratio of nylon to filler is 1:0.3.

[0022] In step (3), the temperature of the first stretching roller is 50° C., and the stretching ratio is 12; the stretching ratio of the second stretching roller is 8, and the laser heating power is 1.2W.

[0023] Embodiment 2:

[0024] The filler is only needle-shaped, and the rest is the same as in Example 1.

[0025] Embodiment 3:

[0026] The filler is only spherical, and the rest is the same as in Example 1.

[0027] Comparative Example 1:

[0028] Laser-assisted heating is not used, and the rest is the same as in Example 1.

[0029] Comparative Example 2:

[0030] The concentration of nylon in the spinning solution in step (2) is 15 wt.%, and the rest is the same as in Example 1.

[0031] Comparative Example 3:

[0032] The weight ratio of nylon to filler is 1:0.7, and the rest is the same as in Example 1.

[0033] Comparative Example 4:

[0034] The weight ratio of the needle-shaped filler to the spherical filler is 1:0.4, and the rest is the same as in Example 1.

[0035] Comparative Example 5:

[0036] The weight ratio of the needle-shaped filler to the spherical filler is 1:2.2, and the rest is the same as in Example 1.

[0037] The conductive fibers obtained in Examples 1-3 and Comparative Examples 1-5 were tested for their conductive properties and mechanical properties, as shown in the following table:

[0038] Unit resistance Ω / cm Breaking strength cN / dtex Example 1 <![CDATA[10 7 ]]> 2.1 Example 2 <![CDATA[10 9 ]]> 1.9 Example 3 <![CDATA[10 9 ]]> 2.1 Comparative Example 1 <![CDATA[10 8 ]]> 1.8 Comparative Example 2 <![CDATA[10 7 ]]> 1.9 Comparative Example 3 <![CDATA[10 5 ]]> 1.4 Comparative Example 4 <![CDATA[10 8 ]]> 1.9 Comparative Example 5 <![CDATA[10 8 ]]> 2.1

[0039] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing light-colored conductive nylon, characterized in that: The following steps are involved: (1) Weigh a light-colored conductive filler, add it to a formic acid solution, and fully disperse it using an ultrasonic disperser in an ice bath; (2) placing the uniformly dispersed formic acid suspension on a stirrer and stirring rapidly, and at the same time adding nylon chips into the suspension to obtain a spinning solution after complete dissolution; the weight ratio of nylon to filler is 1:0.2-0.6; (3) The spinning solution is added to the screw extruder and extruded, hot air is passed through the spinning tunnel, and high-multiple drawing is achieved through the rapidly rotating first drawing roller. The solvent of the spinning solution is continuously volatilized during the drawing process, and the fiber is formed and wound on the first drawing roller. The fiber is then quickly heated by a laser-assisted heating method and is drawn twice through the second drawing roller to obtain a light-colored conductive nylon. The concentration of nylon in the spinning solution in step (2) is 15-35wt.%; The light-colored conductive filler in step (1) is at least one of conductive TiO2 and conductive potassium titanate having a core-shell structure, the shell layer of the light-colored conductive filler is a conductive component, the composition is at least one of antimony-doped tin oxide, tin-doped indium oxide, and aluminum-doped zinc oxide, and the diameter is within 250nm; The filler is a spherical and needle-shaped blended conductive filler with a weight ratio of 1:0.5-2.

2. According to the method for preparing light-colored conductive nylon according to claim 1, in step (3), the temperature of the first drafting roller is 40-60°C, and the drafting ratio is 8-15; the drafting ratio of the second drafting roller is 6-12, and the laser heating power is 1.2W.