A photocatalyst CuNi / CN and its preparation method and application
By in-situ synthesis of CuNi/CN composite catalysts on carbon nitride nanosheets, the problems of insufficient light absorption and charge mobility of carbon nitride photocatalysts are solved, the photocatalytic performance and hydrogen production efficiency are significantly improved, and efficient hydrogen and Production of fine chemicals.
Patent Information
- Application Number
- CN202310367174.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Existing carbon nitride (g-C3N4) photocatalysts have deficiencies in light absorption and charge mobility, which limit their photocatalytic performance.
The CuNi/CN composite catalyst was prepared using an in-situ synthesis method. By combining copper and nickel complexes with carbon nitride nanosheets, a bimetallic supported catalyst was formed, which improved the photocatalytic activity and hydrogen production efficiency.
It significantly improves the photocatalytic activity and hydrogen production efficiency of the benzyl alcohol dehydrogenation reaction, broadens the light absorption range, accelerates the separation and migration of photogenerated electrons and holes, and achieves efficient production of hydrogen and fine chemicals.
Smart Images

Figure CN116474807B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photocatalysts, and in particular to a photocatalyst CuNi / CN and a preparation method and application thereof. Background Art
[0002] Hydrogen is an energy source for future industry and human life due to its pollution-free and high energy storage properties. Photocatalytic hydrogen production is an ecological and sustainable method for obtaining H2, so the development of efficient and high-yield photocatalysts is a research hotspot.
[0003] Carbon nitride (g-C3N4) has attracted extensive interdisciplinary attention as a two-dimensional hydrogen production photocatalyst. Although g-C3N4 has suitable conduction and valence band potentials, good thermal stability and large specific surface area, it has weak light absorption and small charge mobility. In recent years, the introduction of bimetallic as co-catalyst has greatly solved these problems.
[0004] The present invention utilizes newly synthesized copper complex and nickel complex to synthesize CuNi / CN composite catalyst in situ, and photocatalytic benzyl alcohol dehydrogenation to produce hydrogen and benzaldehyde is carried out under the action of the composite catalyst. It is found that the CuNi / CN composite catalyst has obvious visible light photocatalytic activity for the dissociation of benzyl alcohol (BA). Compared with pure g-C3N4 (abbreviated as CN) nanosheets, the photocatalytic activity has a qualitative leap, and the hydrogen production efficiency and benzaldehyde (BAD) yield of the best 2% Cu1Ni1 / CN nanocomposite material are greatly improved. This improvement in photocatalytic efficiency can be attributed to the synergistic effect of CuNi bimetallic, which greatly improves the separation efficiency of photogenerated electrons and holes. The impressive properties of CuNi / CN indicate that it has great potential in solar energy conversion applications. Summary of the invention
[0005] The purpose of the present invention is to provide a photocatalyst CuNi / CN and a preparation method and application thereof, which has the advantages that the CuNi / CN composite catalyst has obvious visible light photocatalytic activity for the dehydrogenation of benzyl alcohol, and compared with the traditional pure CN photocatalyst, the CuNi / CN composite catalyst has a significantly improved productivity of photocatalytic dehydrogenation of benzyl alcohol to produce hydrogen and benzaldehyde. The present invention verifies that the rational construction of the noble metal-free composite photocatalytic material realizes the efficient simultaneous photocatalytic production of hydrogen and fine chemicals.
[0006] The above technical objectives of the present invention are achieved through the following technical solutions: A method for preparing a photocatalyst CuNi / CN, comprising the following steps:
[0007] s1: dissolving dicyandiamide and cupric acetate in water and forming a solution after ultrasonic dispersion;
[0008] s2: The solution was transferred to a flask, heated in a water bath at 55-65°C under nitrogen protection, and naturally cooled to room temperature to generate a blue precipitate, which was washed with water several times and then dried to obtain a copper complex;
[0009] s3: Dissolve dicyandiamide in water, add nickel chloride, and obtain a solution after ultrasonic dispersion. Transfer the solution to a flask, add sodium borohydride, heat in a water bath at 75-85°C, and cool naturally to room temperature to generate a green precipitate. Wash three times with water and dry to obtain a nickel complex.
[0010] s4: dissolving dicyandiamide in water to form a solution, adding copper complex and nickel complex, ultrasonically stirring, freezing, and drying to obtain a sample;
[0011] s5: After grinding and mixing the sample and sodium borohydride, calcine at 545-555°C for several hours in a nitrogen atmosphere, and then calcine at 495-505°C for several hours in a hydrogen atmosphere, and then grind, wash with water, wash with HCl, and dry to obtain a CuNi / CN composite catalyst.
[0012] The present invention is further configured such that the molar ratio of dicyandiamide to cupric acetate in s1 is 2:1.
[0013] The present invention is further configured as follows: the water bath heating time in s2 is 4-5 hours.
[0014] The present invention is further configured as follows: the molar ratio of dicyandiamide to nickel chloride in s3 is 3:2.
[0015] The present invention is further configured as follows: in s4, the mass ratio of the copper complex to the nickel complex is in the range of 1:0.5-2.
[0016] The present invention is further configured as follows: the calcination time at 545-555° C. in s5 is 3.8-4.2 h, and the heating rate is 4-5° C. / min.
[0017] The present invention is further configured as follows: the calcination time at 495-505°C in an S5 hydrogen atmosphere is 4.8-5.2 hours, and the heating rate is 4-5°C / min.
[0018] The photocatalyst CuNi / CN is obtained by the preparation method.
[0019] The photocatalyst CuNi / CN is used in preparing hydrogen and benzaldehyde from benzyl alcohol.
[0020] In summary, the present invention uses an in-situ synthesis method of a bimetallic complex to manufacture a bimetallic composite catalyst supported on carbon nitride as an advanced photocatalyst for the dehydrogenation reaction of benzyl alcohol to produce benzaldehyde and H2. Carbon nitride nanosheets provide an instantaneous charge transfer pathway, while the supported bimetallic CuNi provides abundant active sites. The intimate interfacial contact between the carbon nitride nanosheets and the CuNi bimetallic catalyst greatly improves its photocatalytic efficiency. Moreover, the bimetallic CuNi broadens the light absorption range, accelerates the separation and migration efficiency of photogenerated carriers, and significantly improves the photocatalytic performance. The composite photocatalyst 2% Cu1Ni1 / CN exhibits high activity (80μmolg -1 h -1 ) and selectivity for the dehydrogenation of aromatic alcohols, and has a higher H2 generation efficiency than traditional CN. The present invention verifies that the rational construction of noble metal-free composite photocatalytic materials enables the efficient simultaneous production of hydrogen and fine chemicals by visible light photocatalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 (a) is the SEM spectrum of CN of Example 1 of the present invention, (b) is the SEM spectrum of 2%Cu1Ni1 / CN, (c) is the HRTEM spectrum of 2%Cu1Ni1 / CN, (d) is the HAADF-STEM image of 2%Cu1Ni1 / CN, (eh) is the element mapping of 2%Cu1Ni1 / CN;
[0022] Figure 2 are XRD spectra of CN, 2%Cu1Ni1 / CN, 2%Cu / CN and 2%Ni / CN of Example 1 of the present invention;
[0023] Figure 3 FTIR spectra of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN of Example 1 of the present invention;
[0024] Figure 4 (a) is the nitrogen adsorption-desorption isotherm and pore size distribution of 2% Cu1Ni1 / CN of Example 1 of the present invention, (b) is the nitrogen adsorption-desorption isotherm and pore size distribution of CN;
[0025] Figure 5 (a) is the C1sXPS spectrum of the CN and 2%Cu1Ni1 / CN composite of Example 1 of the present invention, (b) the N1sXPS spectrum of the CN and 2%Cu1Ni1 / CN composite, (c) the Cu2p spectrum of the 2%Cu1Ni1 / CN composite, the inset is the CuLMM spectrum, (d) the Ni2pXPS spectrum of the 2%Cu1Ni1 / CN composite;
[0026] Figure 6(a) is the electrochemical impedance Nyquist spectrum of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN of Example 1 of the present invention, (b) is the instantaneous photocurrent response of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN;
[0027] Figure 7 (a) is the UV-visible diffuse reflectance spectra of CN and 2%Cu1Ni1 / CN of Example 1 and the test example of the present invention, (b) the relationship between the transformed Kubelka-Munk function of CN and 2%Cu1Ni1 / CN and the light energy, (c) the Mott-Schottky curves of CN and 2%Cu1Ni1 / CN, (d) the band gap diagram of CN and 2%Cu1Ni1 / CN;
[0028] Figure 8 are steady-state photoluminescence spectra of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN of Example 1 and the test example of the present invention;
[0029] Fig. 9 (a) is the catalytic efficiency of different ratios of bimetallic CuNi in Examples 1-5 of the present invention and the test example, (b) is the catalytic efficiency of different mass ratios of CuNi bimetallic and CN, (c) is the cycle test of the photocatalytic hydrogen production performance of the 2% Cu1Ni1 / CN sample, (d) is the XRD test of the 2% Cu1Ni1 / CN sample before and after the cycle;
[0030] Fig.10 The electron spin paramagnetic resonance spectra of CN and 2% Cu1Ni1 / CN composite photocatalysts of Example 1 and Test Example of the present invention under visible light irradiation and without visible light irradiation;
[0031] Fig.11 (a) is the redox reaction in the photocatalytic process of Example 1 and the test example of the present invention, and (b) is a schematic diagram of the photocatalytic benzaldehyde synthesis and H2 generation in the composite material 2% Cu1Ni1 / CN. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with the accompanying drawings.
[0033] Embodiment 1:
[0034] A method for preparing a photocatalyst CuNi / CN comprises the following steps:
[0035] (1) Synthesis steps of copper complex:
[0036] Dissolve dicyandiamide (20 mmol, 1.6816 g) and copper acetate (10 mmol, 1.9965 g) in 40 mL of water, and quickly form a uniform solution after ultrasonic treatment. Transfer the uniform solution to a three-necked flask and then heat it in a water bath at 60 ° C for 5 h under nitrogen protection. After cooling naturally to room temperature, wash the blue precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0037] (2) Nickel complex formation steps:
[0038] Dissolve dicyandiamide (30mmol, 2.523g) in 100mL of water, then add nickel chloride (4.734g, 20mmol) to the solution, ultrasonicate to form a uniform solution, and transfer to a flask. Dissolve sodium borohydride (0.05g) in 1mL of water, slowly add it dropwise to the above uniform solution, and heat it in a water bath at 80°C for 3h. After cooling naturally to room temperature, wash the green precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0039] (3) Preparation steps of CuNi / CN composite catalyst:
[0040] 2g of dicyandiamide was dissolved in 20mL of water to form a clear and transparent uniform solution, and then 0.04g of copper complex and nickel complex were added to the above solution and ultrasonically stirred to make the complex uniformly dispersed. Then the uniformly dispersed solution was quickly placed in liquid nitrogen for freezing, and finally placed in a vacuum dryer for drying. The dried sample and sodium borohydride were ground and mixed evenly, and calcined at 550℃ for 4h (heating rate 5℃ / min) in a tube furnace in a nitrogen atmosphere, and then calcined at 500℃ for 5 hours (heating rate 5℃ / min) in a hydrogen atmosphere. After the reaction was completed, it was ground, washed with water 3 times, and then washed with HCl to remove the oxides on the composite catalyst. Finally, it was placed in a vacuum dryer for drying to obtain a sample 2% Cu1Ni1 / CN composite catalyst (copper complex: nickel complex: dicyandiamide mass ratio = 1:1:50, 1 / 50 = 2%, so it is called 2% Cu1Ni1 / CN), which was named Cu1Ni1 / CN.
[0041] Embodiment 2:
[0042] A method for preparing a photocatalyst CuNi / CN comprises the following steps:
[0043] (1) Synthesis steps of copper complex:
[0044] Dissolve dicyandiamide (20 mmol, 1.6816 g) and copper acetate (10 mmol, 1.9965 g) in 40 mL of water, and quickly form a uniform solution after ultrasonic treatment. Transfer the uniform solution to a three-necked flask and then heat it in a water bath at 60 ° C for 5 h under nitrogen protection. After cooling naturally to room temperature, wash the blue precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0045] (2) Nickel complex formation steps:
[0046] Dissolve dicyandiamide (30mmol, 2.523g) in 100mL of water, then add nickel chloride (4.734g, 20mmol) to the solution, ultrasonicate to form a uniform solution, and transfer to a flask. Dissolve sodium borohydride (0.05g) in 1mL of water, slowly add it dropwise to the above uniform solution, and heat it in a water bath at 80°C for 3h. After cooling naturally to room temperature, wash the green precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0047] (3) Preparation steps of CuNi / CN composite catalyst:
[0048] Dissolve 2g of dicyandiamide in 20mL of water to form a clear and transparent uniform solution, then take 0.04g of copper complex and 0.06g of nickel complex respectively, add them to the above solution and perform ultrasonic stirring to make the complex dispersed evenly. Then quickly put the evenly dispersed solution into liquid nitrogen for freezing, and finally put it into a vacuum dryer for drying. Take the dried sample and sodium borohydride, grind and mix evenly, and use a tube furnace to calcine at 550℃ in a nitrogen atmosphere for 4h (heating rate 5℃ / min), then calcine at 500℃ in a hydrogen atmosphere for 5 hours (heating rate 5℃ / min), grind after the reaction is completed, wash with water 3 times, and then wash with HCl to remove the oxides on the composite catalyst. Finally, put it into a vacuum dryer for drying to obtain a sample of 2%Cu1Ni 1.5 / CN composite catalyst, named Cu1Ni 1.5 / CN.
[0049] Embodiment 3:
[0050] A method for preparing a photocatalyst CuNi / CN comprises the following steps:
[0051] (1) Synthesis steps of copper complex:
[0052] Dissolve dicyandiamide (20 mmol, 1.6816 g) and copper acetate (10 mmol, 1.9965 g) in 40 mL of water, and quickly form a uniform solution after ultrasonic treatment. Transfer the uniform solution to a three-necked flask and then heat it in a water bath at 60 ° C for 5 h under nitrogen protection. After cooling naturally to room temperature, wash the blue precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0053] (2) Nickel complex formation steps:
[0054] Dissolve dicyandiamide (30mmol, 2.523g) in 100mL of water, then add nickel chloride (4.734g, 20mmol) to the solution, ultrasonicate to form a uniform solution, and transfer to a flask. Dissolve sodium borohydride (0.05g) in 1mL of water, slowly add it dropwise to the above uniform solution, and heat it in a water bath at 80°C for 3h. After cooling naturally to room temperature, wash the green precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0055] (3) Preparation steps of CuNi / CN composite catalyst:
[0056] 2g of dicyandiamide was dissolved in 20mL of water to form a clear and transparent uniform solution, and then 0.04g of copper complex and 0.08g of nickel complex were added to the above solution and ultrasonically stirred to make the complex uniformly dispersed. Then the uniformly dispersed solution was quickly placed in liquid nitrogen for freezing, and finally placed in a vacuum dryer for drying. The dried sample and sodium borohydride were ground and mixed uniformly, and calcined at 550°C for 4h (heating rate 5°C / min) in a tubular furnace in a nitrogen atmosphere, and then calcined at 500°C for 5 hours (heating rate 5°C / min) in a hydrogen atmosphere. After the reaction was completed, the sample was ground, washed with water 3 times, and then washed with HCl to remove the oxide on the composite catalyst. Finally, it was placed in a vacuum dryer for drying to obtain a sample 2% Cu1Ni2 / CN composite catalyst, which was named Cu1Ni2 / CN.
[0057] Embodiment 4:
[0058] A method for preparing a photocatalyst CuNi / CN comprises the following steps:
[0059] (1) Synthesis steps of copper complex:
[0060] Dissolve dicyandiamide (20 mmol, 1.6816 g) and copper acetate (10 mmol, 1.9965 g) in 40 mL of water, and quickly form a uniform solution after ultrasonic treatment. Transfer the uniform solution to a three-necked flask and then heat it in a water bath at 60 ° C for 5 h under nitrogen protection. After cooling naturally to room temperature, wash the blue precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0061] (2) Nickel complex formation steps:
[0062] Dissolve dicyandiamide (30mmol, 2.523g) in 100mL of water, then add nickel chloride (4.734g, 20mmol) to the solution, ultrasonicate to form a uniform solution, and transfer to a flask. Dissolve sodium borohydride (0.05g) in 1mL of water, slowly add it dropwise to the above uniform solution, and heat it in a water bath at 80°C for 3h. After cooling naturally to room temperature, wash the green precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0063] (3) Preparation steps of CuNi / CN composite catalyst:
[0064] Dissolve 2g of dicyandiamide in 20mL of water to form a clear and transparent uniform solution, then take 0.06g of copper complex and 0.04g of nickel complex respectively, add them to the above solution and perform ultrasonic stirring to make the complex evenly dispersed. Then quickly put the evenly dispersed solution into liquid nitrogen for freezing, and finally put it into a vacuum dryer for drying. Take the dried sample and sodium borohydride, grind and mix evenly, and use a tube furnace to calcine at 550℃ in a nitrogen atmosphere for 4h (heating rate 5℃ / min), then calcine at 500℃ in a hydrogen atmosphere for 5 hours (heating rate 5℃ / min), grind after the reaction, wash with water 3 times, and then wash with HCl to remove the oxides on the composite catalyst. Finally, put it into a vacuum dryer for drying to obtain a sample of 2% Cu 1.5 The Ni1 / CN composite catalyst was named Cu 1.5 Ni1 / CN.
[0065] Embodiment 5:
[0066] A method for preparing a photocatalyst CuNi / CN comprises the following steps:
[0067] (1) Synthesis steps of copper complex:
[0068] Dissolve dicyandiamide (20 mmol, 1.6816 g) and copper acetate (10 mmol, 1.9965 g) in 40 mL of water, and quickly form a uniform solution after ultrasonic treatment. Transfer the uniform solution to a three-necked flask and then heat it in a water bath at 60 ° C for 5 h under nitrogen protection. After cooling naturally to room temperature, wash the blue precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0069] (2) Nickel complex formation steps:
[0070] Dissolve dicyandiamide (30mmol, 2.523g) in 100mL of water, then add nickel chloride (4.734g, 20mmol) to the solution, ultrasonicate to form a uniform solution, and transfer to a flask. Dissolve sodium borohydride (0.05g) in 1mL of water, slowly add it dropwise to the above uniform solution, and heat it in a water bath at 80°C for 3h. After cooling naturally to room temperature, wash the green precipitate produced by the reaction with water three times. Finally, collect the precipitate and dry it in a freeze dryer;
[0071] (3) Preparation steps of CuNi / CN composite catalyst:
[0072] 2g of dicyandiamide was dissolved in 20mL of water to form a clear and transparent uniform solution. Then 0.08g of copper complex and 0.04g of nickel complex were added to the above solution and ultrasonically stirred to make the complex uniformly dispersed. Then the uniformly dispersed solution was quickly put into liquid nitrogen for freezing, and finally put into a vacuum dryer for drying. The dried sample and sodium borohydride were ground and mixed uniformly, and calcined at 550°C for 4h (heating rate 5°C / min) in a tubular furnace in a nitrogen atmosphere, and then calcined at 500°C for 5 hours (heating rate 5°C / min) in a hydrogen atmosphere. After the reaction was completed, the sample was ground, washed with water 3 times, and then washed with HCl to remove the oxide on the composite catalyst. Finally, it was put into a vacuum dryer for drying to obtain a sample 2% Cu2Ni1 / CN composite catalyst, which was named Cu2Ni1 / CN.
[0073] Figure 1 (a) is the SEM spectrum of CN of Example 1 of the present invention, (b) is the SEM spectrum of 2% Cu1Ni1 / CN, (c) is the HRTEM spectrum of 2% Cu1Ni1 / CN, (d) is the HAADF-STEM image of 2% Cu1Ni1 / CN, (eh) is the element mapping of 2% Cu1Ni1 / CN. It can be seen from the figure that the Cu and Ni elements are evenly distributed without obvious separation, indicating that the CuNi bimetallic is successfully and evenly dispersedly loaded on CN;
[0074] Figure 2The XRD spectra of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN in Example 1 of the present invention show that the basic skeleton structure of CN is well maintained after metal loading;
[0075] Figure 3 FTIR spectra of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN of Example 1 of the present invention, from which it can be seen that the CN structure is well retained after metal loading;
[0076] Figure 4 (a) is the nitrogen adsorption-desorption isotherm and pore size distribution of 2% Cu1Ni1 / CN of Example 1 of the present invention, (b) is the nitrogen adsorption-desorption isotherm and pore size distribution of CN. It can be seen from the figure that CuNi metal is successfully loaded on the nanorods, and it is proved that the specific surface area is not the main factor in enhancing hydrogen production;
[0077] Figure 5 (a) is the C1s spectrum of the CN and 2% Cu1Ni1 / CN complex of Example 1 of the present invention, (b) is the N1s spectrum of the CN and 2% Cu1Ni1 / CN complex, (c) is the Cu2p spectrum of the 2% Cu1Ni1 / CN complex, and the inset is the CuLMM spectrum, (d) is the Ni2p spectrum of the 2% Cu1Ni1 / CN complex. It can be seen from (a) and (b) that there is a strong interaction between the CuNi bimetallic and CN, and the CuNi bimetallic co-catalyst has a strong attraction for electrons, which helps to regulate the transport behavior of photogenerated electrons. It can be seen from (c) and (d) that the CuNi bimetallic is successfully loaded on the CN nanosheets;
[0078] Figure 6 (a) is the electrochemical impedance Nyquist spectrum of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN in Example 1 of the present invention, (b) is the instantaneous photocurrent response of CN, 2% Cu1Ni1 / CN, 2% Cu / CN and 2% Ni / CN. It can be seen from the figure that the CuNi bimetallic co-catalyst can significantly accelerate charge separation and transport.
[0079] Test example:
[0080] 1. Optical absorption test: The 2% Cu1Ni1 / CN catalyst of Example 1 was subjected to an optical absorption test. The test results are as follows: Figure 7 As shown, specifically as Figure 7As shown in a, the UV-visible absorption spectrum of the 2%Cu1Ni1 / CN catalyst was further studied. Compared with CN, the 2%Cu1Ni1 / CN catalyst sample showed a clear absorption edge near 470nm, and the absorption increased in the entire spectral range, which indicates that the introduction of bimetallic can broaden the light absorption range of the catalyst. The bandgap width of CN and 2%Cu1Ni1 / CN was estimated using the KM method, as shown in Figure 7 As shown in b, the calculated band gap values of CN and 2%Cu1Ni1 / CN are 2.75eV and 2.65eV. The positions of the conduction bands of CN and 2%Cu1Ni1 / CN can be determined from the MottSchottky plot, as shown in Figure 7 c, which shows that the flat band potentials of CN and 2% Cu1Ni1 / CN were measured to be −1.21 V and −1.31 V (vs. Ag / AgCl), respectively, and the conduction band position (vs. NHE) was obtained by shifting the flat band potential to −0.1 V. Figure 7 d shows the band gap changes of CN and 2%Cu1Ni1 / CN. The Cu-Ni bimetallic cocatalyst narrows the band gap of CN, improves the positions of the conduction band and valence band, and promotes the catalyst to absorb the adsorbed H + Ability to be reduced to H2.
[0081] 2. Steady-state photoluminescence spectrum test: The 2% Cu1Ni1 / CN catalyst of Example 1 was subjected to spectrum test. The test results are as follows: Figure 8 As shown, specifically Figure 8 The PL spectra of CN, 2% Cu / CN, 2% Ni / CN and 2% Cu1Ni1 / CN at an excitation wavelength of 350nm are shown. All samples have emission peaks at 450nm, and the emission peak of pure CN is the highest, indicating that the photogenerated carriers in CN are strongly composited. The copper-nickel bimetallic co-catalyst acts as a charge carrier capture center, which can extract the photogenerated electrons in CN to the interface between the two, and then quickly reach the active point of the co-catalyst. Therefore, the emission peak of 2% Cu1Ni1 / CN is the lowest, indicating that the combination of photogenerated electron-hole pairs in 2% Cu1Ni1 / CN is greatly suppressed, which greatly promotes the photocatalytic reaction.
[0082] 3. Photocatalytic performance test: The 2% Cu1Ni1 / CN catalysts of Examples 1-5 were subjected to photocatalytic tests. The catalytic performance was evaluated by the photocatalytic hydrogen evolution rate under vacuum conditions. The test results are shown in Table 1. Fig. 9 As shown, specifically Fig. 9 a compares the catalytic efficiency of bimetallic Cu and Ni at different mass ratios. From the figure, we can see that as the mass ratio of metal Cu and Ni increases, the catalytic efficiency of the composite catalyst is not as high as the efficiency with a mass ratio of 1:1. The results show that when the mass ratio of CuNi bimetallic is 1:1, the photocatalytic efficiency of the composite catalyst reaches the maximum. Fig. 9 b shows the comparison of the catalytic efficiency of CuNi bimetallic and CN at different mass ratios (where the mass ratio of Cu and Ni is fixed at 1:1). Pure CN shows a H2 productivity of 0.15 μmol h -1 g -1 , which is caused by the shortage of active sites and the rapid recombination of photogenerated carriers. After loading the CuNi bimetallic, the H2 generation efficiency increased significantly, and a volcano-type relationship between the CuNi loading and the product yield was observed. When the CuNi loading was 2%, the composite photocatalyst showed the best benzyl alcohol (BA) conversion activity (78.9 μmol g -1 h -1 ) and H2 release (80 μmol g -1 h -1 ); with the increase of the ratio, the catalytic efficiency showed an increase from 0.5% to 2%, and then a decrease from 2% to 4%. In general, 2% Cu1Ni1 / CN showed the best catalytic efficiency; when the molar ratio exceeded 2%, the photocatalytic efficiency decreased, which may be due to the fact that the active centers on the CN surface were covered by excess CuNi metal. At the same time, the analysis of the liquid products showed that the main conversion product was benzaldehyde (BAD), and no signals of other products were observed. The generation rate of BAD is almost proportional to the generation rate of H2, which indicates that the generation of BAD is highly selective and the BA conversion rate of the best sample 2% Cu1Ni1 / CN reached 73%, as shown in the table below. The stability of the photocatalyst is also an important parameter that needs to be studied, such as Fig. 9 As shown in Figure c, the four-day cycle experiment showed that the hydrogen production efficiency remained stable, indicating that the composite material was reusable without obvious activity loss, indicating that the stability of the 2%Cu1Ni1 / CN photocatalyst was high. Fig. 9 d is the XRD spectrum of the composite catalyst 2% Cu1Ni1 / CN before and after the cycle. It can be clearly seen that there is no significant difference between the catalyst and before the reaction, which further confirms its good cycle stability.
[0083]
[0084] 4. Exploration of the mechanism of catalytic reaction Test: The 2% Cu1Ni1 / CN catalyst of Example 1 was subjected to quenching experiment and electron spin paramagnetic resonance spectroscopy analysis experiment in sequence. The test results are shown in the following table and Fig.10 As shown:
[0085]
[0086] The reaction conditions in the table are 40 mL BA and 20 mg 2% Cu1Ni1 / CN catalyst. N2 gas atmosphere, irradiation for 3 hours; 0.1 mmol quencher; TEOA bstands for triethanolamine (hole scavenger). CCl4 c represents carbon tetrachloride (electron scavenger). As shown in the table, when the hole scavenger triethanolamine (TEOA) was added to the reaction system, BAD (168.6 μmol g -1 ) was severely inhibited, while the generation rate of H2 remained basically unchanged. The above results indicate that in the photocatalytic system, the holes generated by light are consumed to carry out the oxidation of BA. Similarly, after adding the electron scavenger carbon tetrachloride (CCl4), the generation rate of H2 was greatly reduced (54.70 μmol g -1 ), indicating that photogenerated electrons are indispensable for the reduction reaction.
[0087] To further verify the generation of free radicals, we conducted electron spin paramagnetic resonance spectroscopy (EPR) analysis experiments. Fig.10 As shown in Figure 2, when 5,5-dimethyl-1-pyrroline N-oxide (DMPO) was used as a free radical scavenger, both blank carbon nitride (CN) and the composite catalyst 2% Cu1Ni1 / CN induced carbon-centered free radicals (α-hydroxybenzyl radical, C α ), indicating that the CH bond on benzyl alcohol was activated by light under illumination. It is worth noting that DMPO-C α The signal intensity of the free radicals is much higher than that of blank carbon nitride (CN), which means that the rates of CH activation and dehydrogenation are greatly accelerated in the presence of CuNi bimetallic.
[0088] Based on the above test results, a reasonable photocatalytic mechanism of 2%Cu1Ni1 / CN composite material was proposed. Fig.11 As shown in Figure 2, under the irradiation of visible light, carbon nitride (CN) is photoexcited to generate electron-hole pairs. The active holes will be quickly captured by the aromatic alcohol adsorbed on the surface, thereby oxidizing the CH bonds and generating C α Free radicals and protons. Then, the photogenerated holes further oxidize C α The free radicals generate aldehydes and release more protons. At the same time, electrons are transferred to the CuNi bimetallic, which easily reacts with protons extracted from the dehydrogenation of benzyl alcohol (BA). Protons are extracted from the dehydrogenation of BA and H2 is produced. The CuNi bimetallic supported on CN has abundant active sites and low hydrogen reduction overpotential, which not only improves charge separation but also promotes surface hydrogen reduction, thereby achieving higher photocatalytic activity than carbon nitride.
[0089] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
Claims
1. A method for preparing a photocatalyst CuNi / CN, characterized in that: The steps include: s1: dissolving dicyandiamide and cupric acetate in water and forming a solution after ultrasonic dispersion; s2: The solution was transferred to a flask, heated in a water bath at 55-65°C under nitrogen protection, and naturally cooled to room temperature to generate a blue precipitate, which was washed with water several times and then dried to obtain a copper complex; s3: Dissolve dicyandiamide in water, add nickel chloride, and obtain a solution after ultrasonic dispersion. Transfer the solution to a flask, add sodium borohydride, heat in a water bath at 75-85°C, and cool naturally to room temperature to generate a green precipitate. Wash three times with water and dry to obtain a nickel complex. s4: dissolving dicyandiamide in water to form a solution, adding copper complex and nickel complex, ultrasonically stirring, freezing, and drying to obtain a sample; s5: After grinding and mixing the sample and sodium borohydride, calcine at 545-555°C for several hours in a nitrogen atmosphere, and then calcine at 495-505°C for several hours in a hydrogen atmosphere, and then grind, wash with water, wash with HCl, and dry to obtain a CuNi / CN composite catalyst.
2. The method for preparing a photocatalyst CuNi / CN according to claim 1, characterized in that: The molar ratio of dicyandiamide to cupric acetate in s1 is 2:
1.
3. The method for preparing a photocatalyst CuNi / CN according to claim 1, characterized in that: The water bath heating time in s2 is 4-5 h.
4. The method for preparing a photocatalyst CuNi / CN according to claim 1, characterized in that: The molar ratio of dicyandiamide to nickel chloride in s3 is 3:
2.
5. The method for preparing a photocatalyst CuNi / CN according to claim 1, characterized in that: The mass ratio of the copper complex to the nickel complex in s4 ranges from 1:0.5 to 2.
6. The method for preparing a photocatalyst CuNi / CN according to claim 1, characterized in that: The calcination time at 545-555°C in s5 is 3.8-4.2 h, and the heating rate is 4-5°C / min.
7. The method for preparing a photocatalyst CuNi / CN according to claim 1, characterized in that: The calcination time at 495-505°C in s5 hydrogen atmosphere is 4.8-5.2h, and the heating rate is 4-5°C / min.
8. The photocatalyst CuNi / CN obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the photocatalyst CuNi / CN according to claim 8 in preparing hydrogen and benzaldehyde from benzyl alcohol.
Citation Information
Patent Citations
Graphene-supported copper-nickel composite nanometer photocatalyst, and preparation method and application thereof
CN104028272A
Strong-reducing-property visible light response photocatalyst with urea and ferric chloride as raw materials
CN105170172A
Preparation method and application of composite photocatalysis material
CN107335460A
Preparation method and application of non-noble metal monoatomic catalyst
CN110449176A
Composite photocatalyst and preparation method thereof
CN111036269A