A flame retardant polypropylene material and preparation method thereof
Through the compounding of black phosphorus and inorganic magnesium and the synergistic effect of organic magnesium and polyacrylamide, the problem of balancing the flame retardant performance and mechanical properties of polypropylene is solved, and efficient flame retardant performance improvement and mechanical properties maintenance are achieved.
Patent Information
- Application Number
- CN202310108194.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-14
AI Technical Summary
When existing technology improves the flame retardant properties of polypropylene, it often leads to a reduction in mechanical properties. Especially in the case of high addition amounts, it is difficult to meet the requirements of flame retardant properties and mechanical properties at the same time.
Black phosphorus and inorganic magnesium are compounded, and organic magnesium compounds and polyacrylamide are introduced to synergistically improve the flame retardant properties while reducing the impact of black phosphorus on mechanical properties. Flame retardant polypropylene materials are prepared through high-speed mixing and extrusion processes.
It effectively improves the flame retardant properties of polypropylene while maintaining or improving its mechanical properties, reducing the negative impact of the addition of inorganic magnesium on the mechanical properties, and further optimizing the flame retardant and mechanical properties of the material through the addition of polyacrylamide.
Smart Images

Figure BDA0004075770570000041 
Figure BDA0004075770570000042 
Figure BDA0004075770570000051
Abstract
Description
Technical Field
[0001] The invention relates to the field of flame retardant materials, in particular to a flame retardant polypropylene material and a preparation method thereof. Background Art
[0002] Black phosphorus is widely known for flame retardant, for example, CN112552579A discloses an organic double-coated black phosphorus nanosheet synergistic halogen-free flame retardant polyethylene composition and its preparation method. The raw material formula of the polyethylene composition is composed of the following components by mass percentage: 42.0% to 50.0% of linear low-density polyethylene, 3.0% to 8.0% of ethylene-methyl acrylate copolymer or ethylene-butyl acrylate copolymer, 35.0% to 45.0% of metal hydroxide, 3.0% to 10.0% of organic double-coated black phosphorus nanosheet, 0.2% to 0.5% of lubricant and 0.1% to 0.3% of antioxidant. The present invention uses polyvinyl pyrrolidone and polyhydroxy Schiff base organic double-coated black phosphorus nanosheets to synergistically flame retard metal hydroxide into linear low-density polyethylene. When the amount of black phosphorus nanosheets is as low as 0.2wt% and the total amount of flame retardant is less than 50wt%, the polyethylene composition passes the V-0 grade of UL-94 flame retardancy, and has high strength and toughness, which can well meet the needs of wire and cable materials.
[0003] CN112011147A discloses a long glass fiber reinforced flame retardant ABS composite material and its preparation method, which includes components such as polycarbonate, ABS, flame retardant, modified fiber, modified graphene oxide, etc., wherein the surface of the modified graphene oxide is treated with a silane coupling agent to improve the compatibility of graphene oxide and matrix components (polycarbonate, ABS), so that it can be evenly dispersed in the system; the modified fiber is mainly prepared by black phosphorene, dopamine, anhydrous ethanol, and pretreated fiber; the pretreated fiber is a glass fiber with carbon nanowires grown on the surface, and the glass fiber is a continuous glass fiber. The synergistic effect of aluminum hydroxide, magnesium hydroxide, polysiloxane, modified graphene oxide and black phosphorene is used to make the ABS composite material have excellent flame retardant properties, and low smoke and low toxicity when burning, and higher practicality.
[0004] PP (polypropylene) is a flammable material with an oxygen index of about 18.
[0005] After research, we found that the use of black phosphorus can improve the flame retardant properties of PP, but the improvement ability is limited.
[0006] Further research found that the flame retardant properties of polypropylene can be improved by compounding magnesium hydroxide and black phosphorus. However, the amount of magnesium hydroxide added must reach more than 15wt% to achieve a better synergistic flame retardant effect. Under the premise of high addition, the mechanical properties are significantly reduced.
[0007] Therefore, the technical problem solved in this case is: how to improve the flame retardant properties of the polypropylene substrate while ensuring the reliability of the mechanical properties. Summary of the invention
[0008] The object of the present invention is to provide a flame-retardant polypropylene material. The material adopts a compound of black phosphorus and inorganic magnesium to improve the flame retardant performance. The use of organic magnesium can further improve the flame retardant performance and the strength of the polypropylene material. The organic magnesium contains hydroxyl groups and can cooperate with black phosphorus to reduce the influence of black phosphorus on the mechanical properties of the system.
[0009] At the same time, the invention also discloses a preparation method of the flame-retardant polypropylene material.
[0010] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a flame retardant polypropylene material, comprising polypropylene, an inorganic magnesium compound, an organic magnesium compound, and black phosphorus; wherein the content of black phosphorus is 6-15wt%; the content of the inorganic magnesium compound is 10-15wt%, and the content of the organic magnesium compound is 5-10wt%; the remainder is polypropylene.
[0011] In some embodiments of the present invention, the amount of black phosphorus can be selected as 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%;
[0012] In some embodiments of the present invention, the amount of the inorganic magnesium compound can be selected to be 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%;
[0013] In some embodiments of the present invention, the amount of the organomagnesium compound can be selected to be 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%;
[0014] As a further preferred embodiment of the present invention, 2-5 wt% of polyacrylamide is also included.
[0015] In the present invention, polyacrylamide has two functions. On the one hand, polyacrylamide can release nitrogen at high temperature to reduce the oxygen concentration near the fire source. On the other hand, polyacrylamide has strong water solubility and can be effectively combined with organic magnesium compounds and polypropylene at the same time to improve the flame retardant properties and mechanical properties of the system.
[0016] As a preferred embodiment of the present invention, it includes polypropylene, inorganic magnesium compound, organic magnesium compound, black phosphorus and polyacrylamide; wherein the content of black phosphorus is 9-12wt%; the content of inorganic magnesium compound is 10-15wt%, organic magnesium compound is 5-8wt%, polyacrylamide is 2-4wt%, and polypropylene is the balance.
[0017] In the flame-retardant polypropylene material, the inorganic magnesium compound is magnesium hydroxide or magnesium oxide; the organic magnesium is hydrated magnesium citrate, magnesium glycinate, magnesium gluconate or magnesium L-aspartate.
[0018] At the same time, the present invention also discloses a method for preparing the flame retardant polypropylene material, comprising the following steps:
[0019] 1) Weigh appropriate amounts of polypropylene resin and organic magnesium compound, and stir them in a high-speed stirrer for 30 minutes to obtain organic magnesium-adhered polypropylene resin;
[0020] 2) Then, add the inorganic magnesium hydroxide compound and black phosphorus to the organic magnesium-adhered polypropylene resin and continue stirring in a high-speed mixer for 30 minutes.
[0021] 3) Pour the premix into a twin-screw extruder, extrude, draw strands and pelletize at a temperature of 200-230° C. and a rotation speed of 100-400 rpm to obtain a flame-retardant polypropylene material.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention uses inorganic magnesium and black phosphorus to add to polypropylene, which can improve the flame retardant properties of polypropylene, but it is also accompanied by a decrease in the mechanical properties of polypropylene. By replacing part of the inorganic magnesium with organic magnesium, the flame retardant properties can be maintained while reducing the deterioration of the mechanical properties.
[0024] The addition of organic magnesium compounds can adhere to the resin surface after high-speed stirring, which is beneficial to the subsequent adhesion of powdered inorganic matter, reduces dusting, and promotes the dispersion function of inorganic powder.
[0025] As a further optimization of the present invention, the flame retardant properties of organic magnesium can be further improved by introducing polyacrylamide, and at the same time, it can cooperate with organic magnesium to further reduce the deterioration of mechanical properties. DETAILED DESCRIPTION
[0026] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0027] Example
[0028] A method for preparing a flame retardant polypropylene material comprises the following steps:
[0029] 1) Weigh appropriate amounts of polypropylene resin and organic magnesium compound, and stir them in a high-speed stirrer for 30 minutes to obtain organic magnesium-adhered polypropylene resin;
[0030] 2) Then, add inorganic magnesium hydroxide compound, black phosphorus, and polyacrylamide (if present) to the organic magnesium-adhered polypropylene resin, and continue stirring in a high-speed mixer for 30 minutes.
[0031] 3) Pour the premix into a twin-screw extruder, extrude, draw strands and pelletize at a temperature of 200-230° C. and a rotation speed of 100-400 rpm to obtain a flame-retardant polypropylene material.
[0032] Among them, the molecular weight of polyacrylamide is 6-13 million, non-ionic, solid content ≥90%, residual monomer is less than 0.2%; hydrolysis degree is 7-8;
[0033] The physical properties of polypropylene are: T30S, parameters: melt flow rate: 3g / 10min, notched impact strength: 39, tensile strength: 32MPa.
[0034] Examples 1-8
[0035] Referring to the preparation method of the embodiment, flame retardant polypropylene was prepared using the formulation shown in Table 1 below.
[0036] Table 1 Recipe
[0037]
[0038] Comparative Examples 1-4
[0039] Referring to the preparation method of the embodiment, flame retardant polypropylene was prepared using the formulation shown in Table 2 below.
[0040] Table 2 Recipe
[0041]
[0042] Performance Testing
[0043] 1. Tensile strength: Use universal tensile testing machine and implement standard 527-2 / T1040.
[0044] 2. Elongation at break: Use universal tensile testing machine and implement standard 527-2 / T1040.
[0045] 3. Impact strength: Use cantilever beam impact testing machine, implement standard 180 / 1A / T1843.
[0046] 4. Oxygen index: Use intelligent oxygen index tester and implement standard GB / T2406.2-2009.
[0047] 5. Flame retardant rating: UL94.
[0048] The test results refer to Table 3;
[0049] Table 3 Test results
[0050]
[0051] Result analysis:
[0052] 1. By comparing Example 6 with Example 2, it can be seen that when polyacrylamide is present, the mechanical properties and flame retardant properties of the material are improved. The reason is that the introduction of polyacrylamide can further improve the flame retardant properties of organic magnesium, and at the same time, it can cooperate with organic magnesium to further reduce the deterioration of mechanical properties.
[0053] 2. By comparing Example 2 with Comparative Examples 1-2, it can be seen that when there is no organic magnesium, the mechanical properties of the material are significantly reduced. This performance comparison proves that replacing inorganic magnesium with organic magnesium will improve the mechanical properties, but the flame retardant properties are not significantly reduced.
[0054] 3. By comparing Comparative Example 3 with Example 2, it can be seen that if only organic magnesium is used, although the mechanical properties of the material are relatively good, the flame retardant properties cannot meet the standards, because in order to make the flame retardant properties of organic magnesium work, a higher decomposition temperature is required, and the best flame retardant time has passed. In addition, the molecular weight of organic magnesium is large and the magnesium equivalent is small, which further hinders the flame retardant properties.
[0055] 4. By comparing Comparative Example 4 with Examples 2 and 7, it can be seen that without the presence of organic magnesium, organic magnesium cannot be effectively combined with polypropylene and polyacrylamide, and is not beneficial to improving the mechanical properties of the system.
Claims
1. A flame retardant polypropylene material, characterized in that: It includes polypropylene, inorganic magnesium compound, organic magnesium compound and black phosphorus; wherein the content of black phosphorus is 6-15wt%; the content of inorganic magnesium compound is 10-15wt%, the content of organic magnesium compound is 5-8wt%; the balance is polypropylene; The organic magnesium is hydrated magnesium citrate or magnesium glycinate.
2. The flame retardant polypropylene material according to claim 1, characterized in that: It also includes 2-5wt% polyacrylamide.
3. The flame retardant polypropylene material according to claim 1, characterized in that: It includes polypropylene, inorganic magnesium compound, organic magnesium compound, black phosphorus and polyacrylamide; the content of black phosphorus is 9-12wt%; the content of inorganic magnesium compound is 10-15wt%, the content of organic magnesium compound is 5-8wt%, the content of polyacrylamide is 2-4wt% and the balance of polypropylene is.
4. The flame retardant polypropylene material according to any one of claims 1 to 3, characterized in that: The inorganic magnesium compound is magnesium hydroxide or magnesium oxide.