Pure natural non-river mud ramie silk coating preparation and ramie silk coating industrial processing method

By using coating preparations with natural ingredients such as humic acid, fulvic acid and mineral salt, the problem of tight river mud resources in the processing of yarn silk is solved, and a pure natural, black and bright coating with high water washing fastness is achieved. The demand for industrial production is avoided, and the use of chemical products is ensured, and the pure natural characteristics and sustainable production of the products are ensured.

CN116479662BActive Publication Date: 2024-11-19ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310102064.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-13
Publication Date
2024-11-19
Estimated Expiration
2043-02-13

AI Technical Summary

Technical Problem

The processing of yarn silk depends on river mud resources, and the existing coating preparation methods are difficult to maintain the pure natural, healthy and environmentally friendly characteristics of the products, and there is a lack of effective alternatives to meet the needs of industrial large-scale production.

Method used

Using pure natural non-river mud coating preparations composed of natural ingredients such as humic acid, fulvic acid and mineral salts, the physicochemical properties similar to those of traditional shisha silk production are formed, and the black and shiny are achieved through specific formulas and process conditions. And a coating with high water-fastness.

Benefits of technology

Overcome the essential defects of chemical synthetic products, realize the industrial production of pure natural and non-river mud coating preparations, have the style and quality similar to traditional craft products, get rid of regional and resource limitations, and meet the sustainability of yarn silk. Production demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116479662B_ABST
    Figure CN116479662B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of classical textile processing, and relates to a pure natural non-river mud ramie silk coating preparation and an industrial processing method of the ramie silk coating. The ingredients of the pure natural non-river mud ramie silk coating preparation are as follows: humic acid, fulvic acid, alum, green vitriol, sodium phytate, starch, carrageenan and water. The coating preparation is applied to the dark surface of the sun-dried ramie fabric by a roller coater, and is left to stand for 30±5 minutes under set environmental conditions, and then washed with water to remove the preparation that is not combined with the sun-dried ramie fabric to obtain a coated fabric. The method of the present invention can obtain a product with a style and quality similar to that of traditional ramie silk.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textile processing, and relates to a pure natural non-river mud ramie silk coating preparation and an industrial processing method of the ramie silk coating. Background Art

[0002] Ramie silk is a natural coated silk product that is unique to my country and has a special fabric style and is comfortable to wear. It feels smooth, soft and crisp, has good moisture permeability and air permeability, and has high color fastness. The processing technology of ramie silk is a national intangible cultural heritage. It is made of all-natural raw materials and manual craftsmanship, but it can only be produced in a very few areas such as Shunde, Foshan. One of the main reasons is that the river mud raw materials required to process the black coating of ramie silk are very special, and its main components and properties are different from those of river mud in other regions. After ramie silk is made into clothing, it is cool and comfortable to wear, and is very suitable for summer wear. The special fabric style and performance of ramie silk originate from its special processing method, namely: the silk fabric is first repeatedly dipped in ramie dye solution and exposed to the sun. The product obtained in this step is named sun-sun ramie fabric (generally the thickness of the sun-sun ramie fabric is 0.2-1.2mm), and its color is dark brown red (such as Figure 1 Then, the dark side of the fabric after sunbathing is coated with river mud, and after sufficient reaction, the floating mud is washed off, and a layer of black and bright pure natural coating is formed on the surface of the fabric (as shown in the left picture). Figure 1 ).

[0003] At present, with the continuous dredging and silk making over the years, the river and pond mud resources that meet the processing requirements of ramie silk processing areas are becoming increasingly scarce. Relying on natural river mud resources and backward production methods do not meet the concept of modern industrialized large-scale production and consumer demand. Therefore, the industry urgently needs natural and effective coating preparations to meet the sustainable production of ramie silk.

[0004] At present, there are few reports on the preparation methods of ramie silk coating, mainly including mud coating method (patent CN102733182B), surface chemical polymerization method (patent CN 114892398 A) and chemical product printing method. These methods either fail to get rid of the limitation of relying on river mud, or use a large amount of chemical synthetic products, which changes the "pure natural", "healthy" and "environmentally friendly" characteristics of ramie silk and is difficult to be accepted by consumers. The ramie silk coating is not only pure natural, with black and bright characteristics, but also has high water fastness, which has high requirements for the properties of the coating preparation that replaces river mud, especially the requirement of "pure natural", which is the basic condition for the industry and consumers to judge the authenticity of ramie silk. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a pure natural non-river mud ramie silk coating preparation and a coating processing method.

[0006] In order to solve the above technical problems, the present invention provides a pure natural non-river mud ramie silk coating preparation, which is composed of the following components in mass percentage:

[0007]

[0008] The balance is water.

[0009] Note: Alum and green vitriol are mineral salts; starch and carrageenan are molding agents. It is common knowledge that humic acid and fulvic acid can be derived from weathered coal, lignite, peat, soil, compost, etc.

[0010] As an improvement of the pure natural non-river mud ramie silk coating preparation of the present invention:

[0011] The average molecular weight of the humic acid is 5 kDa to 30 kDa (tested by gel permeation chromatography);

[0012] The humic acid was prepared into an aqueous solution with a concentration of 0.10 mg / mL, and the absorbance at 253 nm and 203 nm was recorded as humic acid, 253 , rot A 203 , rot A 253 / rot A 203 =1.58~1.68; that is, humic acid must contain abundant oxygen-containing groups such as phenolic hydroxyl and carboxyl.

[0013] Humic acid 253 The ratio to its concentration (mg / mL) is 11.0-15.0; that is, the humic acid needs to have a higher degree of aromatization.

[0014] As a further improvement of the pure natural non-river mud ramie silk coating preparation of the present invention:

[0015] The average molecular weight of fulvic acid is 0.5 kDa to 2 kDa (measured by gel permeation chromatography).

[0016] The fulvic acid was prepared into an aqueous solution with a concentration of 0.10 mg / mL, and the absorbance at 253 nm and 203 nm was recorded as fulvic acid A and fulvic acid B, respectively. 253 , Rich A 203 , Rich A 253 / richA 203 =0.40~0.60; that is, fulvic acid must contain abundant oxygen-containing groups such as phenolic hydroxyl and carboxyl.

[0017] Rich A in fulvic acid 253 The ratio to its concentration (mg / mL) is 11.5 to 14.5; that is, fulvic acid needs to have a higher degree of aromatization.

[0018] The present invention also provides a method for processing a ramie silk coating, using the above-mentioned pure natural non-river mud ramie silk coating preparation, comprising the following steps:

[0019] The components of the coating preparation (pure natural non-river mud ramie silk coating preparation) are dissolved, stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric using a roller coater, and allowed to stand for 30±5 minutes under set environmental conditions, and then washed with water to remove the preparation that has not combined with the sun-dried fabric (i.e., has not reacted), thereby obtaining a coated fabric.

[0020] As an improvement of the processing method of the ramie silk coating of the present invention: in the ramie silk coating processing method, the mass ratio of coating preparation: ramie silk after sun-drying is 2:1 to 10:1.

[0021] As a further improvement of the processing method of the camisole silk coating of the present invention, the set environmental conditions in the processing method of the camisole silk coating are: an environmental temperature of 20 to 70° C. and an environmental relative humidity of 60 to 95%.

[0022] The principle of the present invention is to use a natural industrial product with a structure and properties similar to the effective components of river mud used in the production of ramie silk, and use the specific formula of the present invention to make the coating preparation have the physical and chemical properties of river mud used in the production of ramie silk. Then, the present invention uses the corresponding industrial production equipment and process to process a product with properties similar to fully handmade ramie silk.

[0023] The present invention fully considers the following contents during the invention process:

[0024] To achieve the goal of forming a black and shiny coating with high washing fastness on the surface of the fabric after sun-drying, it is first necessary to select a preparation similar to the effective ingredient of "black mud" used in the production of handmade ramie silk, that is, humic acid. Since humic acid is a large category of products, it has a wide range of sources and very different properties. The molecular weight and degree of aromatization of humic acid determine its degree of "blackness", while the active groups such as hydroxyl and carboxyl groups on the structure of humic acid determine its ability to form colloids and the fastness of binding to the surface of the fabric, that is, the ability to form a firm coating on the surface of the fabric. The source of fulvic acid is similar to that of humic acid, and its color is lighter. It mainly plays the role of bonding humic acid into granules, while mineral salts play the role of consolidating humic acid, fulvic acid and fabric into one through chelation, which is the key to improving the fastness of the coating. In addition, a molding agent is also required to facilitate the machinery and equipment to finish the above effective ingredients on the surface of the fabric through processing methods such as scraping and roller coating.

[0025] The invention uses humic acid, fulvic acid, mineral salt and molding agent of suitable sources, structures and proportions, and a certain post-finishing method to prepare a product similar to the traditional process ramie silk by using a pure natural, non-river mud compound preparation.

[0026] Compared with the prior art, the present invention has the following positive effects:

[0027] First, the coating preparation is obtained by using natural industrial products with structures and properties similar to river mud used in the production of ramie silk. The raw materials are purely natural, which overcomes the essential defects of the current industry's large-scale use of "imitation products" processed from chemical synthetic products;

[0028] Secondly, the chemical reaction properties of this coating preparation are similar to those of natural river mud. The ramie silk coating obtained by processing is black and shiny, and the surface effect is similar to that of ramie silk products produced by traditional river mud processing.

[0029] Thirdly, the ingredients of the coating preparation are widely available and inexpensive, and more importantly, they are not limited to river mud, thus breaking away from the geographical and resource limitations of ramie silk production.

[0030] In summary, the present invention discloses a coating formulation that can replace river mud used in traditional ramie silk production, which is composed of commercially available products that are natural or derived from natural products. By selecting suitable key components, humic acid and fulvic acid, and processing them with the specific formulation of the present invention and corresponding process conditions, a product with a style and quality similar to that of traditional ramie silk can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 These are sun-dried ramie fabrics (shown in dark brown in the color picture) and traditional ramie silk products (shown in black in the color picture) processed with river mud.

[0032] Figure 2 The fabric is the fabric in Example 1 of the present invention which is washed 5 times before and after processing.

[0033] Figure 3 The fabric is the fabric processed in Example 2 of the present invention and the fabric washed 5 times.

[0034] Figure 4 The fabric is the fabric processed in Example 3 of the present invention and the fabric washed 5 times.

[0035] Figure 5 The fabric is the fabric processed in Example 4 of the present invention and the fabric washed 5 times.

[0036] Figure 6 The fabric is the fabric processed in Example 5 of the present invention and the fabric washed 5 times.

[0037] Figure 7 This is the fabric processed in Comparative Example 1-1 of the present invention.

[0038] Figure 8 The fabric is the fabric processed in Comparative Example 1-2 of the present invention and the fabric washed 5 times.

[0039] Fig. 9 This is the fabric processed in Comparative Example 2-1 of the present invention.

[0040] Fig.10 This is the fabric obtained by processing in Comparative Example 3-1 of the present invention.

[0041] Fig.11 This is the fabric obtained by processing in Comparative Example 3-2 of the present invention.

[0042] Fig.12 This is the fabric obtained by processing in Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0043] The following cases all use the same sun-dried fabric, and the thickness of the sun-dried fabric is about 0.45mm.

[0044] The coating preparation is prepared and used for the processing of ramie silk coating.

[0045] It should be emphasized that the humic acid and fulvic acid used in the present invention only need to meet the conditions set by the present invention. Therefore, products from different manufacturers can be selected as needed, and can even be extracted and specially prepared from sources such as soil, peat, and lignite mines as required.

[0046] Embodiment 1:

[0047] 1) Prepare a pure natural non-river mud ramie silk coating preparation, the formula (ingredients and composition) of which is:

[0048]

[0049] The balance is water.

[0050] The above proportions are all mass percentages.

[0051] The humic and fulvic acids in the formula are:

[0052] Humic acid: The absorbance of 0.1 mg / mL humic acid aqueous solution at 253 nm is 253 =1.47, absorbance at 203nm 203 =0.91. Therefore, 253 / rot A 203 =1.62; rot A 253 / Its concentration (mg / mL) = 14.7; the average molecular weight measured by gel permeation chromatography = 12.5 kDa. The humic acid can be purchased from Shandong Agricultural University Fertilizer Technology Co., Ltd. (extracted from lignite mine).

[0053] Fulvic acid: The absorbance of 0.1 mg / mL fulvic acid aqueous solution at 253 nm is 253 =1.30, absorbance at 203nm is rich in A203 =2.66. Therefore, rich A 253 / richA 203 =0.49; Rich A 253 / Its concentration (mg / mL) = 13.0; Average molecular weight measured by gel permeation chromatography = 1.0 kDa. The fulvic acid can be purchased from Shandong Agricultural University Fertilizer Technology Co., Ltd. (extracted from lignite mine).

[0054] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0055] According to the formula of the coating preparation described in 1), the coating preparation is dissolved and stirred evenly, and after being completely gelatinized (stirring at a speed of about 60 rpm for 5 minutes can achieve complete gelatinization), the coating preparation is applied to the dark surface of the sun-dried fabric by a roller coater at a mass ratio of 5:1 (i.e., the mass ratio of coating preparation: sun-dried fabric = 5:1), and is allowed to stand for 30 minutes under environmental conditions of a temperature of 29° C. and a relative humidity of 68%, and then washed with water to remove the preparation that has not been combined with the sun-dried fabric (i.e., has not reacted), to obtain a coated fabric.

[0056] The obtained ramie silk fabric is as follows Figure 2 The results are analyzed as follows:

[0057] Compared with before processing, the fabric becomes black and shiny. According to the conventional spectrophotometer, the color depth K / S value is as high as 12.03. Visually, the black coating completely covers the original reddish brown of the fabric, showing an obvious coating, and the color and coating are uniform (such as Figure 2 As shown in the figure, it is a typical ramie silk appearance style. According to the AATCC Assessment Procedure 9 "Visual Assessment of Color Difference of Textiles", the color difference reaches 5 levels (color difference is divided into 0-5 levels, the higher the level, the smaller the color difference); according to GB / T12490-2007 "Textiles - Color Fastness Tests - Color Fastness to Home and Commercial Washing", the fabric coating's color fastness to washing reaches 4 levels, which is excellent.

[0058] The detection basis of the following cases is the same as that of Example 1.

[0059] Embodiment 2:

[0060] 1) The formula of the pure natural non-river mud ramie silk coating preparation is the same as that of Example 1;

[0061] The humic acid and fulvic acid in this case formula are:

[0062] Humic acid: The absorbance of 0.1 mg / mL humic acid aqueous solution at 253 nm is 253 =1.34, absorbance at 203nm 203 =0.80. Therefore,253 / rot A 203 =1.67; rotten A 253 / Its concentration (mg / mL) = 13.4; average molecular weight = 21.0 kDa. It can be purchased from Shandong Agricultural University Fertilizer Technology Co., Ltd. (extracted from lignite mine, belongs to active humic acid).

[0063] Fulvic acid: The absorbance of 0.1 mg / mL fulvic acid aqueous solution at 253 nm is 253 =1.18, absorbance at 203nm is rich in A 203 =2.03. Therefore, rich A 253 / richA 203 =0.58; Rich A 253 / Its concentration (mg / mL) = 11.8; average molecular weight = 0.7 kDa. It can be purchased from Shanghai Yuanye Biotechnology Co., Ltd. (extracted from soil).

[0064] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0065] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 3:1 using a roller coater, and allowed to stand for 30 minutes under environmental conditions of a temperature of 29° C. and a relative humidity of 68%, and then washed with water to remove the unreacted preparation to obtain a coated fabric.

[0066] The obtained ramie silk fabric is as follows Figure 3 The results are analyzed as follows:

[0067] Compared with before processing, the fabric becomes black and shiny. The color depth K / S value is as high as 11.88 when tested with a conventional spectrophotometer. Visual inspection of the sample shows obvious coating, and the color and coating are uniform (see Figure 3 ), with a typical ramie silk appearance style. Its color difference reaches level 5; the color fastness to washing of the fabric coating reaches level 4, with excellent color fastness to washing.

[0068] Embodiment 3:

[0069] 1) The formula of the pure natural non-river mud ramie silk coating preparation is the same as that of Example 1;

[0070] The humic acid and fulvic acid in this case formula are:

[0071] Humic acid: The absorbance of 0.1 mg / mL humic acid aqueous solution at 253 nm is 253 =1.16, absorbance at 203nm 203 =0.73. Therefore, 253 / rot A 203=1.59; rotten A 253 / Its concentration (mg / mL) = 11.6; average molecular weight = 5.3 kDa. Humic acid can be purchased from Pingxiang Hongtu Humic Acid Co., Ltd. (derived from compost fermentation).

[0072] Fulvic acid: The absorbance of 0.10 mg / mL fulvic acid aqueous solution at 253 nm is 253 =1.44, absorbance at 203nm is rich in A 203 =3.32. Therefore, rich A 253 / richA 203 =0.43; Rich A 253 / Its concentration (mg / mL) = 14.4; Average molecular weight = 0.5 kDa. The above fulvic acid can be purchased from Shandong Jingfeng Humic Acid Technology Co., Ltd. (derived from peat).

[0073] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0074] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 2:1 using a roller coater, and allowed to stand for 30 minutes under environmental conditions of a temperature of 29° C. and a relative humidity of 68%, and then the unreacted preparation is washed off with water to obtain a coated fabric.

[0075] The obtained ramie silk fabric is as follows Figure 4 The results are analyzed as follows:

[0076] Compared with before processing, the fabric becomes black and shiny. The color depth K / S value is as high as 11.70 when tested with a conventional spectrophotometer. Visual inspection of the sample shows obvious coating, and the color and coating are relatively uniform (see Figure 4 ), which is a typical appearance style of ramie silk. Its color difference reaches level 4; the color fastness to washing of the fabric coating is level 3, and the color uniformity and color fastness to washing meet the commercial requirements.

[0077] Embodiment 4:

[0078] 1) The formula of the pure natural non-river mud ramie silk coating preparation is the same as that of Example 1;

[0079] The humic acid and fulvic acid in this case formula are:

[0080] Humic acid: The absorbance of 0.1 mg / mL humic acid aqueous solution at 253 nm is 253 =1.12, absorbance at 203nm 203 =0.68. Therefore, 253 / rot A 203 =1.65; rot A 253 / Its concentration (mg / mL) = 11.2; Average molecular weight = 28.3 kDa. The above humic acid can be purchased from Shandong Jingfeng Humic Acid Technology Co., Ltd. (derived from peat).

[0081] Fulvic acid: The absorbance of 0.1 mg / mL fulvic acid aqueous solution at 253 nm is 253 =1.22, absorbance at 203nm is rich in A 203 =2.21. Therefore, rich A 253 / richA 203 =0.55; Rich A 253 / Its concentration (mg / mL) = 12.2; Average molecular weight = 1.9 kDa. Fulvic acid can be purchased from Xi'an Virgin Biotechnology Co., Ltd. (Shilajit extract).

[0082] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0083] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 10:1 using a roller coater, and allowed to stand for 30 minutes under environmental conditions of a temperature of 29° C. and a relative humidity of 68%, and then the unreacted preparation is washed off with water to obtain a coated fabric.

[0084] The obtained ramie silk fabric is as follows Figure 5 The results are analyzed as follows:

[0085] Compared with before processing, the fabric becomes black and shiny. According to the conventional spectrophotometer, the color depth K / S value is as high as 11.04. Visual inspection shows that the black coating completely covers the original reddish brown of the fabric, showing obvious coating, and the color and coating are uniform (such as Figure 5 The color difference of the fabric reaches level 4; the color fastness to washing of the fabric coating is level 4, which is excellent.

[0086] Embodiment 5:

[0087] 1) The formula of the pure natural non-river mud ramie silk coating preparation is the same as that of Example 1;

[0088] The humic acid and fulvic acid in this case formula are:

[0089] Humic acid: The absorbance of 0.1 mg / mL humic acid aqueous solution at 253 nm is 253 =1.15, absorbance at 203nm 203 =0.71. Therefore, 253 / rot A 203 =1.62; rot A 253 / Its concentration (mg / mL) = 11.5; Average molecular weight = 7.3 kDa. The above humic acid can be purchased from Lingshi County Linhai Humic Acid Factory (derived from lignite mine).

[0090] Fulvic acid: The absorbance of 0.1 mg / mL fulvic acid aqueous solution at 253 nm is 253 =1.24, absorbance at 203nm is rich in A 203 =2.34. Therefore, rich A 253 / richA 203 =0.53; Rich A 253 / Its concentration (mg / mL) = 12.4; Average molecular weight = 1.1 kDa. The above fulvic acid can be purchased from Shizuishan Haiyuan Chemical Plant (derived from weathered coal).

[0091] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0092] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 7:1 using a roller coater, and allowed to stand for 30 minutes under environmental conditions of a temperature of 29° C. and a relative humidity of 68%, and then the unreacted preparation is washed off with water to obtain a coated fabric.

[0093] The obtained ramie silk fabric is as follows Figure 6 The results are analyzed as follows:

[0094] Compared with before processing, the fabric becomes black and shiny. The color depth K / S value is as high as 11.37 when tested with a conventional spectrophotometer. Visual inspection shows that the black coating completely covers the original reddish brown color of the fabric, indicating an obvious coating, and the color and coating are uniform (see Figure 6 ), which is a typical appearance style of ramie silk. Its color difference reaches level 4; the color fastness to washing of the fabric coating is level 3, and the color difference and color fastness to washing meet the commercial requirements.

[0095] Embodiment 6:

[0096] 1) Prepare a pure natural non-river mud ramie silk coating preparation, the formula of which is:

[0097]

[0098]

[0099] The balance is water.

[0100] The above proportions are all mass percentages.

[0101] Humic acid and fulvic acid are the same as those used in Example 1.

[0102] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0103] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 5:1 using a roller coater, and allowed to stand for 30 minutes under environmental conditions of a temperature of 30° C. and a relative humidity of 65%, and then washed with water to remove the unreacted preparation to obtain a coated fabric.

[0104] The results are analyzed as follows:

[0105] Compared with the original fabric, the prepared ramie silk becomes black and shiny, with a color depth K / S value of up to 13.75, showing an obvious coating, and the color and coating are relatively uniform, with a typical ramie silk appearance style. Its color difference reaches level 4; the color fastness to washing of the fabric coating reaches level 3, and the color uniformity and color fastness to washing meet the commercial requirements.

[0106] Embodiment 7:

[0107] 1) Prepare a pure natural non-river mud ramie silk coating preparation, the formula of which is:

[0108]

[0109] The balance is water.

[0110] The above proportions are all mass percentages.

[0111] Humic acid and fulvic acid are the same as those used in Example 1.

[0112] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0113] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 5:1 using a roller coater, and is allowed to stand in a constant temperature and humidity chamber at a temperature of 40° C. and a relative humidity of 70% for 30 minutes, and then washed with water to remove the unreacted preparation to obtain a coated fabric.

[0114] The results are analyzed as follows:

[0115] Compared with the original fabric, the prepared ramie silk fabric becomes black and shiny, with a color depth K / S value of up to 10.98, showing an obvious coating, and the color and coating are uniform, with a typical ramie silk appearance style. Its color difference reaches level 5; the color fastness to washing of the fabric coating reaches level 4, and the color uniformity and color fastness to washing are both excellent.

[0116] Embodiment 8:

[0117] 1) Prepare a pure natural non-river mud ramie silk coating preparation, the formula of which is:

[0118]

[0119] The balance is water.

[0120] The above proportions are all mass percentages.

[0121] Humic acid and fulvic acid are the same as those used in Example 1.

[0122] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0123] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 5:1 using a roller coater, and is allowed to stand in a constant temperature and humidity chamber at a temperature of 50° C. and a relative humidity of 80% for 30 minutes, and then washed with water to remove the unreacted preparation to obtain a coated fabric.

[0124] The results are analyzed as follows:

[0125] Compared with the original fabric, the prepared ramie silk fabric becomes black and shiny, with a color depth K / S value of up to 11.54, showing an obvious coating, and the color and coating are uniform, with a typical ramie silk appearance style. Its color difference reaches level 4; the color fastness to washing of the fabric coating reaches level 4, and the color uniformity and color fastness to washing are both good.

[0126] Embodiment 9:

[0127] 1) Prepare a pure natural non-river mud ramie silk coating preparation, the formula of which is:

[0128]

[0129] The balance is water.

[0130] The above proportions are all mass percentages.

[0131] Humic acid and fulvic acid are the same as those used in Example 1.

[0132] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0133] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 5:1 using a roller coater, and is allowed to stand in a constant temperature and humidity chamber at a temperature of 65° C. and a relative humidity of 90% for 30 minutes, and then washed with water to remove the unreacted preparation to obtain a coated fabric.

[0134] The results are analyzed as follows:

[0135] Compared with the original fabric, the prepared ramie silk fabric becomes black and shiny, with a color depth K / S value of up to 10.79, showing an obvious coating, and the color and coating are uniform, with a typical ramie silk appearance style. Its color difference reaches level 3; the color fastness to washing of the fabric coating reaches level 3, and the color uniformity and color fastness to washing meet the commercial requirements.

[0136] Embodiment 10:

[0137] 1) Prepare a pure natural non-river mud ramie silk coating preparation, the formula of which is:

[0138]

[0139]

[0140] The balance is water.

[0141] The above proportions are all mass percentages.

[0142] Humic acid and fulvic acid are the same as those used in Example 1.

[0143] 2) Processing the coating of the ramie silk in the following manner, comprising:

[0144] The coating preparation described in 1) is dissolved and stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric at a mass ratio of 5:1 using a roller coater, and is allowed to stand in a constant temperature and humidity chamber at a temperature of 70° C. and a relative humidity of 65% for 30 minutes, and then washed with water to remove the unreacted preparation to obtain a coated fabric.

[0145] The results are analyzed as follows:

[0146] Compared with the original fabric, the prepared ramie silk fabric becomes black and shiny, with a color depth K / S value of up to 13.88, showing an obvious coating, and the color and coating are uniform, with a typical ramie silk appearance style. Its color difference reaches level 4; the color fastness to washing of the fabric coating reaches level 3, and the color uniformity and color fastness to washing meet the commercial requirements.

[0147] Comparative Example 1-1,

[0148] The humic acid in Example 1 is changed as follows, and the rest is the same as Example 1.

[0149] The absorbance of 0.1 mg / mL humic acid aqueous solution at 253 nm is 253 =0.97, absorbance at 203nm 203 =0.61, then: Corrosion A 253 / rot A 203 =1.59, rotten A 253 / Its concentration (mg / mL) = 9.7. Average molecular weight = 3.1 kDa. The humic acid can be purchased from Shengjiayou Biotechnology Development Co., Ltd. (extracted from river and pond sediment).

[0150] The aromaticity and molecular weight of the humic acid are relatively low and do not meet the range specified in the present invention.

[0151] The results are analyzed as follows:

[0152] The resulting fabric is Figure 7 As shown. The fabric color depth is obviously shallow, far from the "black and shiny" level of ramie silk, and the coating is not significant enough, the color difference is level 1, and the fabric color depth K / S value is only 9.2, far from meeting the commercial requirements. It can be seen that humic acid with an aromatization degree and molecular weight lower than that specified in the present invention is not suitable for processing ramie silk.

[0153] Comparative Example 1-2

[0154] The humic acid in Example 1 is changed as follows, and the rest is the same as Example 1.

[0155] The absorbance of 0.1 mg / mL humic acid aqueous solution at 253 nm is 253 =1.59, the absorption at 203nm 203 =1.04, then: Corrosion A 253 / rot A 203 =1.53, rot A 253 / Its concentration (mg / mL) = 15.9. Average molecular weight = 35.6 kDa. The humic acid can be purchased from Shijiazhuang Chunfeng Biotechnology Co., Ltd. (derived from biomass compost fermentation).

[0156] The aroma degree and molecular weight of the humic acid are too high and do not meet the range specified in the present invention.

[0157] The results are analyzed as follows:

[0158] The resulting fabric is Figure 8 As shown in the figure, the K / S value of the fabric is as high as 14.22, and the appearance is as black and shiny as the ramie silk. However, the coating quality of the fabric is low, the coating is hard, brittle, and uneven, and the color difference is only level 2; the black coating of the fabric falls off significantly after washing, and the color fastness to washing is only level 1. The requirements for color difference and color fastness to washing (generally level 3 and above) for the commercialization of general textiles are not met. It can be seen that humic acid with a higher degree of aromatization and molecular weight than that specified in the present invention is not suitable for processing ramie silk.

[0159] Comparative Example 2-1

[0160] The fulvic acid in Example 2 is changed as follows, and the rest is the same as Example 2.

[0161] The absorbance of 0.1 mg / mL fulvic acid aqueous solution at 253 nm is 253 =1.06, the absorbance at 203nm is rich in A 203 =3.17, then: Rich A 253 / richA 203 =0.33, A 253 / Its concentration (mg / mL) = 10.6. Average molecular weight = 1.1 kDa. The fulvic acid can be purchased from Hubei Kewode Chemical Co., Ltd. (extracted from river and pond sediment).

[0162] The number of oxygen-containing active groups in the fulvic acid component is relatively small and does not meet the scope specified in the present invention.

[0163] The results are analyzed as follows:

[0164] The resulting fabric is Fig. 9 As shown, the K / S value of the fabric is 10.75, the fabric color and coating are uneven, the color difference is only 2 levels, and the coating quality of the fabric is also low, which obviously does not meet the product requirements. It can be seen that the fulvic acid with a significantly smaller number of oxygen-containing groups than that specified in the present invention is not suitable for processing ramie silk.

[0165] Comparative Example 2-2

[0166] The fulvic acid in Example 2 is changed as follows, and the rest is the same as Example 2.

[0167] The absorbance of 0.1 mg / mL fulvic acid aqueous solution at 253 nm is 253 =1.18, the absorbance at 203nm is rich in A 203 =2.61, then: Rich A 253 / richA 203 =0.45, Rich A 253 / Its concentration (mg / mL) = 11.8. Average molecular weight = 0.2 kDa. Fulvic acid can be purchased from Shandong Ruihongze Chemical Technology Co., Ltd. (from lignite mine).

[0168] The molecular weight of the fulvic acid is relatively small and does not meet the range specified in the present invention.

[0169] The results are analyzed as follows:

[0170] The K / S value of the prepared fabric is 10.87, the fabric color and coating are obviously uneven, the coating quality of the fabric is low, the color difference of the fabric is level 1, and the color fastness to washing is only level 2, which does not meet the product requirements. It can be seen that fulvic acid whose molecular weight does not meet the requirements of the present invention is not suitable for processing ramie silk.

[0171] Comparative Example 3-1

[0172] The alum and green vitriol in Example 4 were replaced by 1% ferrous sulfate (ie, 1% ferrous sulfate simultaneously replaced 0.12% alum and 0.10% green vitriol). The rest was the same as Example 4.

[0173] The results are analyzed as follows:

[0174] The resulting coating preparation has a more obvious granular feel. Fig.10 As shown, the color and coating of the fabric are very uneven, the color difference is level 0, and it does not meet the product requirements.

[0175] Comparative Example 3-2

[0176] The content of alum in Example 4 is reduced to 0.01%, and the content of green vitriol is reduced to 0.015%. The rest is the same as Example 4.

[0177] The results are analyzed as follows:

[0178] The resulting fabric is Fig.11 As shown, the fabric color and coating are uneven, and the color difference is level 1, which does not meet the product requirements.

[0179] Comparative Example 3-3

[0180] The content of alum in Example 4 was increased to 0.35%, and the content of green vitriol was increased to 0.5%. The rest was the same as Example 4.

[0181] The results are analyzed as follows:

[0182] The coating of the prepared fabric is not uniform enough, the surface of the fabric is uneven, the color difference is level 2, the appearance quality of the fabric is low, and it does not meet the commercial requirements.

[0183] Comparative Example 4

[0184] The humic acid content in Example 7 was reduced to 2.5%, and the rest was the same as Example 7.

[0185] The results are analyzed as follows:

[0186] The resulting fabric is Fig.12 As shown, the fabric is lighter in color, with a K / S value of only 8.72, uneven color and coating, and a color difference of level 1, which is far from meeting the requirements for productization.

[0187] Comparative Example 5-1

[0188] The starch content in Example 9 was reduced to 12.5%, and the carrageenan content was reduced to 0.2%; the rest was the same as Example 9.

[0189] The results are analyzed as follows:

[0190] The color and coating of the prepared fabric are uneven, the color difference is 2 levels, and the black coating penetrates to the reverse side of the fabric, and the fabric quality does not meet the product requirements.

[0191] Comparative Example 5-2

[0192] The starch content in Example 9 was increased to 30%, and the carrageenan content was increased to 8%; the rest was the same as Example 9.

[0193] The results are analyzed as follows:

[0194] The color of the prepared fabric is lighter, the K / S value is only 9.31, the coating is very thin (the coating is thin and cannot completely cover the red-brown base color, resulting in lower K / S and color uniformity), and the color and coating are not uniform enough, and the color difference is level 2. The fabric quality does not meet the product requirements.

[0195] Comparative Example 6-1

[0196] The mass ratio of the coating preparation to the fabric in Example 3 was reduced to 1.5:1. That is, the amount of the coating preparation used was reduced. The rest was the same as Example 3.

[0197] The results are analyzed as follows:

[0198] The color of the prepared fabric is lighter, the K / S value is only 9.55, the color difference is 2 levels, and the coating is very thin, which is very different from the traditional handmade ramie silk. This is because the amount of coating preparation is too small, it is difficult to apply evenly, and the fabric quality does not meet the product requirements.

[0199] Comparative Example 6-2

[0200] The ambient temperature in Example 3 was lowered to 10° C. The rest was the same as Example 3.

[0201] The results are analyzed as follows:

[0202] The color of the prepared fabric is lighter, the K / S value is only 9.02, the color difference is 2 levels, and the coating is very thin. The quality of the fabric does not meet the product requirements. This is caused by the reaction temperature being too low and the reaction being insufficient.

[0203] Comparative Example 6-3

[0204] The relative humidity of the environment in Example 3 was reduced to 50%. The rest was the same as in Example 3.

[0205] The results are analyzed as follows:

[0206] The coating and color of the prepared fabric are very uneven, with a color difference of 2. The fabric quality does not meet the product requirements. This is because the coating preparation on the surface of the fabric dries too quickly, and the reaction is insufficient and uneven.

[0207] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.

Claims

1. A pure natural non-river mud ramie silk coating preparation, characterized in that It is composed of the following ingredients in percentage by mass: Humic acid 5.0%~16.0% Fulvic acid 2.0%~8.0% Alum 0.02%~0.2% Green vitriol 0.02%~0.2% Sodium phytate 0.5%~5.0% Starch 15.0%~25.0% Carrageenan 0.5%~5.0% The balance is water; The average molecular weight of the humic acid is 5 kDa~30 kDa; the humic acid is prepared into an aqueous solution with a concentration of 0.10 mg / mL, and the absorbance at 253 nm and 203 nm is recorded as humic acid, respectively. 253 , rot A 203 , rot A 253 / rot A 203 =1.58~1.68; Humic acid 253 The ratio to its concentration is 11.0 to 15.0; The average molecular weight of fulvic acid is 0.5 kDa to 2 kDa. The fulvic acid is prepared into an aqueous solution with a concentration of 0.10 mg / mL, and the absorbances at 253 nm and 203 nm are recorded as fulvic acid A and fulvic acid B, respectively. 253 , Rich A 203 , Rich A 253 / richA 203 =0.40~0.60; A-rich fulvic acid 253 The ratio to its concentration is 11.5 to 14.

5.

2. The pure natural non-river mud ramie silk coating preparation according to claim 1, characterized in that It is composed of the following ingredients in percentage by mass: Humic acid 9.5% Fulvic acid 5.5% Alum 0.12% Green vitriol 0.10% Sodium Phytate 2.0% Starch 20.0% Carrageenan 1.5% The balance is water.

3. The pure natural non-river mud ramie silk coating preparation according to claim 2, characterized in that Is any of the following: The average molecular weight of humic acid is 12.5 kDa. 253 / rot A 203 =1.62, rotten A 253 / its concentration = 14.7; the average molecular weight of fulvic acid is 1.0 kDa, rich A 253 / richA 203 =0.49, Rich A 253 / its concentration = 13.0; The average molecular weight of humic acid is 21.0 kDa. 253 / rot A 203 =1.67, rotten A 253 / its concentration = 13.4; the average molecular weight of fulvic acid is 0.7 kDa, rich A 253 / richA 203 =0.58, Rich A 253 / its concentration = 11.8; The average molecular weight of humic acid is 5.3 kDa. 253 / rot A 203 =1.59, rotten A 253 / its concentration = 11.6; the average molecular weight of fulvic acid is 0.5 kDa, rich in A 253 / richA 203 =0.43; Rich A 253 / its concentration = 14.4; The average molecular weight of humic acid is 28.3 kDa. 253 / rot A 203 =1.65; rot A 253 / its concentration = 11.2; the average molecular weight of fulvic acid is 1.9 kDa, rich in A 253 / richA 203 =0.55, Rich A 253 / its concentration = 12.2; Or the average molecular weight of humic acid = 7.3 kDa, humic acid 253 / rot A 203 =1.62; rot A 253 / its concentration = 11.5; average molecular weight of fulvic acid = 1.1 kDa, rich A 253 / richA 203 =0.53; Rich A 253 / Its concentration = 12.

4.

4. The pure natural non-river mud ramie silk coating preparation according to claim 1, characterized in that: The average molecular weight of humic acid is 12.5 kDa. 253 / rot A 203 =1.62, rotten A 253 / its concentration = 14.7; the average molecular weight of fulvic acid is 1.0 kDa, rich A 253 / richA 203 =0.49, Rich A 253 / Its concentration = 13.

0.

5. The pure natural non-river mud ramie silk coating preparation according to claim 4, characterized in that The recipe is any of the following: Humic acid 15.5%, fulvic acid 2.5%, alum 0.03%, green vitriol 0.17%, sodium phytate 0.6%, starch 24.5%, carrageenan 0.7%, the balance is water; Or humic acid 5.5%, fulvic acid 7.5%, alum 0.17%, green vitriol 0.03%, sodium phytate 4.5%, starch 15.5%, carrageenan 4.5%, the balance is water; Or humic acid 7.5%, fulvic acid 6.5%, alum 0.08%, green vitriol 0.08%, sodium phytate 3.5%, starch 17.5%, carrageenan 3.5%, the balance is water; Or humic acid 5.5%, fulvic acid 2.5%, alum 0.03%, green vitriol 0.03%, sodium phytate 0.6%, starch 15.5%, carrageenan 0.7%, the balance is water; Or humic acid 15.5%, fulvic acid 7.5%, alum 0.17%, green vitriol 0.17%, sodium phytate 4.5%, starch 24.5%, carrageenan 4.5%, and the balance is water.

6. A method for processing a camisole silk coating, characterized in that: The method of using the pure natural non-river mud ramie silk coating preparation as claimed in any one of claims 1 to 5 comprises the following steps: The components of the coating preparation are dissolved, stirred evenly, and after being completely gelatinized, the coating preparation is applied to the dark surface of the sun-dried fabric using a roller coater, and allowed to stand for 30±5 minutes under set environmental conditions, and then washed with water to remove the preparation that is not combined with the sun-dried fabric to obtain a coated fabric; Coating preparation: sun-dried fabric = mass ratio of 2:1 to 10:1; The set environmental conditions are: ambient temperature 20~70°C, ambient relative humidity 60~95%.