A polycarboxylate water reducer and preparation method thereof
By using antibacterial modifiers in polycarboxylic acid water reducing agents, combining organic and inorganic antibacterial materials, the antibacterial performance is improved and the spoilage is reduced, the problem of perishable polycarboxylic acid water reducing agents is solved, and the construction of concrete is improved Performance and product stability.
Patent Information
- Application Number
- CN202310439888.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-23
AI Technical Summary
During use, polycarboxylic acid water reducing agents are prone to spoilage and deterioration due to microbial reproduction, affecting product performance.
Using antibacterial modifiers, including antibacterial components, loading components and stable components, by combining antibacterial components with loading components, the overall stability of the antibacterial modifier is improved and the spoilage caused by microbial reproduction is reduced. Deterioration. Antibacterial components include organic antibacterial materials and inorganic antibacterial materials, loading components include linear low-density polyethylene and polyethylene wax, and stabilizing components include hydrophilic nanotitanium dioxide, which improves the stability of antibacterial modifiers through the mixing and preparation process and Dispersion uniformity.
It effectively improves the antibacterial properties of polycarboxylic acid water reducing agents, reduces spoilage and deterioration caused by microbial reproduction, improves the construction performance of concrete, and simplifies the preparation process.
Smart Images

Figure BDA0004193537500000051 
Figure BDA0004193537500000071 
Figure BDA0004193537500000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of concrete admixtures, and more specifically, to a polycarboxylate water reducer and a preparation method thereof. Background Art
[0002] High-performance concrete is one of the key development directions at present. It is gradually gaining favor in the construction market due to its characteristics of fast hardening, high strength and high density. Good fluidity and pumpability are the prerequisites for the safe application of concrete. However, in the process of mixing high-strength concrete, in order to ensure the mechanical properties of concrete, a large amount of adhesive and low water-binder ratio are often used, which leads to problems such as high viscosity and slow flow rate of concrete, which greatly affects the working performance of concrete.
[0003] In order to solve the problem of poor concrete working performance caused by high concrete viscosity, polycarboxylic acid water reducer is widely used in actual projects. Compared with other types of water reducers, it has the advantages of high water reduction rate and small slump loss. At the same time, it can improve the volume stability of concrete and effectively reduce the chance of cracking.
[0004] During use, polycarboxylic acid mother liquor usually needs to be compounded with functional materials such as retarders, water retaining agents and workability regulators. The organic matter such as the compounded polycarboxylic acid mother liquor and other functional materials provides nutrients for the reproduction of microorganisms, which causes the compounded polycarboxylic acid water reducer to rot and deteriorate, thereby causing the product performance to deteriorate. Summary of the invention
[0005] In order to reduce the corruption and deterioration of polycarboxylic acid water-reducing agent caused by microbial growth and reduce the adverse effects on product performance, the present application provides a polycarboxylic acid water-reducing agent and a preparation method thereof.
[0006] In the first aspect, the present application provides a polycarboxylate water reducer, which adopts the following technical solution:
[0007] A polycarboxylate water-reducing agent comprises 60-80 parts of a polycarboxylate water-reducing agent mother liquor, 30-50 parts of a polycarboxylate collapse-preventing agent mother liquor, 24-48 parts of a functional material, 20-30 parts of an antibacterial modifier, and water is added to 1000 parts. The antibacterial modifier comprises an antibacterial component, a load component and a stabilizing component, and the weight ratio of the antibacterial component, the load component and the stabilizing component is 25:1-2:1-3.
[0008] By adopting the above technical solution, the antibacterial component is combined with the load component, and the overall stability of the antibacterial modifier is improved by stabilizing the component, so that the antibacterial performance of the prepared polycarboxylate water-reducing agent is effectively improved, thereby reducing the situation where the polycarboxylate water-reducing agent is corrupted and deteriorated due to microbial reproduction, thereby reducing the adverse effects on product performance.
[0009] Preferably, the antibacterial component comprises an organic antibacterial material and an inorganic antibacterial material, and the weight ratio of the organic antibacterial material to the inorganic antibacterial material is 1:1-3.
[0010] By adopting the above technical solution, the organic antibacterial material and the inorganic antibacterial material are mixed as the antibacterial component, thereby effectively improving the antibacterial performance of the antibacterial modifier.
[0011] Preferably, the organic antibacterial material is catechin and honeysuckle extract, the weight ratio of the catechin and honeysuckle extract is 1:1, and the inorganic antibacterial material is nano copper oxide and nano montmorillonite, the weight ratio of the nano copper oxide and nano montmorillonite is 1:1-5.
[0012] By adopting the above technical scheme, after the antibacterial modifier is evenly mixed with other raw materials, catechins are permeated by water and dissolved in water, thereby improving the antibacterial properties of the polycarboxylic acid water reducer, while the inorganic antibacterial material continues to play an antibacterial role, further improving the antibacterial properties of the polycarboxylic acid water reducer.
[0013] Preferably, the load component includes linear low-density polyethylene and polyethylene wax, and the weight ratio between the two is 19:1.
[0014] By adopting the above technical scheme, linear low-density polyethylene and polyethylene wax are used as raw materials, and the antibacterial component is mixed with the stabilizing component to prepare the antibacterial modifier, thereby effectively improving the overall stability of the antibacterial modifier.
[0015] Preferably, the stabilizing component is hydrophilic nano-titanium dioxide.
[0016] By adopting the above technical scheme, the addition of the stabilizing component improves the density and compactness of the prepared antibacterial modifier on the one hand, and improves the hydrophilicity of the antibacterial modifier on the other hand, making the antibacterial modifier easier to combine with water, facilitating the dissolution of the organic antibacterial material in the antibacterial component in water, and improving the antibacterial properties of the polycarboxylic acid water reducer.
[0017] Preferably, the preparation of the antibacterial modifier comprises the following steps: mixing the antibacterial component, the load component and the stabilizing component, preparing particles by melting, extruding and granulating, and then freezing by liquid nitrogen and crushing, thereby preparing the antibacterial modifier.
[0018] By adopting the above technical solution, thermoplastic plastic is used as a load carrier to combine with the antibacterial component and the stabilizing component, so that the performance of the antibacterial modifier is more stable, and when the antibacterial modifier is mixed with other components, its dispersion uniformity is effectively improved.
[0019] Preferably, the functional material comprises sodium tripolyphosphate, sodium gluconate, sodium thiosulfate and hydroxypropyl methylcellulose, and the weight ratio of the sodium tripolyphosphate, sodium gluconate, sodium thiosulfate and hydroxypropyl methylcellulose is 2:2:3:1.
[0020] By adopting the above technical solution and adding functional materials, the water reducing agent can take into account the functions of retarder, water retaining agent and workability regulator, thereby improving the construction performance of concrete.
[0021] In the second aspect, the present application provides a method for preparing a polycarboxylic acid water reducer, adopting the following technical scheme: a method for preparing a polycarboxylic acid water reducer, comprising the following steps: mixing a polycarboxylic acid water reducer mother liquor, a polycarboxylic acid collapse retaining agent mother liquor, a functional material and an antibacterial modifier, adding water to make up to 1000 parts, stirring and mixing evenly, and sealing to obtain a polycarboxylic acid water reducer.
[0022] By adopting the above technical solution, the mother liquor, functional materials and antibacterial modifier are simply mixed with water to obtain a polycarboxylic acid water reducer with excellent antibacterial performance, and the operation is simple and convenient.
[0023] In summary, this application has the following beneficial effects:
[0024] 1. The addition of the stabilizing component of the present application improves the density and compactness of the prepared antibacterial modifier on the one hand, and improves the hydrophilicity of the antibacterial modifier on the other hand, making the antibacterial modifier easier to combine with water, facilitating the dissolution of the organic antibacterial material in the antibacterial component in water, and improving the antibacterial properties of the polycarboxylic acid water reducer.
[0025] 2. Functional materials are added in this application so that the water reducer can take into account the functions of retarder, water retaining agent and workability regulator, thereby improving the construction performance of concrete.
[0026] 3. The method of the present application can produce a polycarboxylate water-reducing agent with excellent antibacterial properties by simple mixing, and the operation is convenient. DETAILED DESCRIPTION
[0027] In the present application, the mother liquor of polycarboxylate water-reducing agent is purchased from the market; the mother liquor of polycarboxylate slump-preventing agent is purchased from the market; the purity of catechin is 98%, the particle size is 80 mesh, and it is purchased from the market; the honeysuckle extract has a particle size of 80 mesh and is purchased from the market; the nano copper oxide has a particle size of 50nm and is purchased from the market; the nano montmorillonite has a particle size of 100nm and is purchased from the market; the linear low-density polyethylene is purchased from the market; the polyethylene wax is purchased from the market; the hydrophilic nano titanium dioxide has a particle size of 30nm and is purchased from the market, and sodium tripolyphosphate is purchased from the market; the sodium gluconate is purchased from the market; the sodium thiosulfate is purchased from the market; and the hydroxypropyl methylcellulose is purchased from the market.
[0028] The present application is further described in detail below in conjunction with embodiments.
[0029] Preparation Example
[0030] Preparation Example 1
[0031] This preparation example provides an antibacterial modifier, which is prepared by the following steps:
[0032] S1. 95 kg of linear low-density polyethylene, 5 kg of polyethylene wax, 1 kg of catechin, 1 kg of honeysuckle extract, 1 kg of nano copper oxide, 1 kg of nano montmorillonite and 4 kg of hydrophilic nano titanium dioxide were stirred and mixed, and then extruded and granulated by a twin-screw extruder to obtain granules with a particle size of 5 mm.
[0033] S2. Freeze the particles obtained in S1 with liquid nitrogen for 15 minutes, and then crush the particles into 150 meshes to obtain an antibacterial modifier.
[0034] Preparation Example 2
[0035] This preparation example provides an antibacterial modifier, which is prepared by the following steps:
[0036] S1. 95 kg of linear low-density polyethylene, 5 kg of polyethylene wax, 1 kg of catechins, 1 kg of honeysuckle extract, 1 kg of nano copper oxide, 3 kg of nano montmorillonite and 8 kg of hydrophilic nano titanium dioxide were stirred and mixed, and then extruded and granulated by a twin-screw extruder to obtain granules with a particle size of 5 mm.
[0037] S2. Freeze the particles obtained in S1 with liquid nitrogen for 15 minutes, and then crush the particles into 150 meshes to obtain an antibacterial modifier.
[0038] Preparation Example 3
[0039] This preparation example provides an antibacterial modifier, which is prepared by the following steps:
[0040] S1. 95 kg of linear low-density polyethylene, 5 kg of polyethylene wax, 1 kg of catechins, 1 kg of honeysuckle extract, 1 kg of nano copper oxide, 5 kg of nano montmorillonite and 12 kg of hydrophilic nano titanium dioxide were stirred and mixed, and then extruded and granulated by a twin-screw extruder to obtain granules with a particle size of 5 mm.
[0041] S2. Freeze the particles obtained in S1 with liquid nitrogen for 15 minutes, and then crush the particles into 150 meshes to obtain an antibacterial modifier.
[0042] Preparation Example 4
[0043] This preparation example provides an antibacterial modifier, which is prepared by the following steps:
[0044] S1. 95 kg of linear low-density polyethylene, 5 kg of polyethylene wax, 1 kg of catechin, 1 kg of honeysuckle extract, 1 kg of nano copper oxide and 3 kg of nano montmorillonite were stirred and mixed, and then extruded and granulated by a twin-screw extruder to obtain granules with a particle size of 5 mm.
[0045] S2. Freeze the particles obtained in S1 with liquid nitrogen for 15 minutes, and then crush the particles into 150 meshes to obtain an antibacterial modifier.
[0046] Preparation Example 5
[0047] This preparation example provides an antibacterial modifier, which is prepared by the following steps:
[0048] 1 kg of catechin, 1 kg of honeysuckle extract, 1 kg of nano copper oxide, 3 kg of nano montmorillonite and 8 kg of hydrophilic nano titanium dioxide were stirred and mixed to prepare an antibacterial modifier.
[0049] Preparation Example 6
[0050] This preparation example provides an antibacterial modifier, which is prepared by the following steps:
[0051] S1. 95 kg of linear low-density polyethylene and 5 kg of polyethylene wax were stirred and mixed, and then extruded and granulated by a twin-screw extruder. The obtained granules had a particle size of 5 mm.
[0052] S2. Freeze the particles obtained in S1 with liquid nitrogen for 15 minutes, and then crush the particles into 150 meshes to obtain an antibacterial modifier.
[0053] Preparation Example 7
[0054] This preparation example provides an antibacterial modifier, which is prepared by the following steps:
[0055] 1 kg of catechin, 1 kg of honeysuckle extract, 1 kg of nano copper oxide and 3 kg of nano montmorillonite were stirred and mixed to prepare an antibacterial modifier.
[0056] Preparation Example 8
[0057] S1. 95 kg of linear low-density polyethylene, 5 kg of polyethylene wax, 3 kg of catechins, 3 kg of honeysuckle extract and 8 kg of hydrophilic nano-titanium dioxide were stirred and mixed, and then extruded and granulated by a twin-screw extruder. The obtained granules had a particle size of 5 mm.
[0058] S2. Freeze the particles obtained in S1 with liquid nitrogen for 15 minutes, and then crush the particles into 150 meshes to obtain an antibacterial modifier.
[0059] Preparation Example 9
[0060] S1. 95 kg of linear low-density polyethylene, 5 kg of polyethylene wax, 1.5 kg of nano copper oxide, 4.5 kg of nano montmorillonite and 8 kg of hydrophilic nano titanium dioxide were stirred and mixed, and then extruded and granulated by a twin-screw extruder. The obtained particles had a particle size of 5 mm.
[0061] S2. Freeze the particles obtained in S1 with liquid nitrogen for 15 minutes, and then crush the particles into 150 meshes to obtain an antibacterial modifier.
[0062] Table 1 Preparation Example Raw Materials (kg)
[0063]
[0064] Example
[0065] Example 1
[0066] This embodiment provides a polycarboxylate water-reducing agent, which is prepared by the following steps:
[0067] 60 kg of polycarboxylic acid water-reducing agent mother liquor, 30 kg of polycarboxylic acid collapse-preventing agent mother liquor, 6 kg of sodium tripolyphosphate, 6 kg of sodium gluconate, 9 kg of sodium thiosulfate, 3 kg of hydroxypropyl methylcellulose, 20 kg of the antibacterial modifier prepared in Preparation Example 1 and 866 kg of water were stirred and mixed uniformly, and sealed to obtain the polycarboxylic acid water-reducing agent.
[0068] Example 2
[0069] This embodiment provides a polycarboxylate water-reducing agent, which is prepared by the following steps:
[0070] 70 kg of polycarboxylic acid water-reducing agent mother liquor, 40 kg of polycarboxylic acid collapse-preventing agent mother liquor, 9 kg of sodium tripolyphosphate, 9 kg of sodium gluconate, 13.5 kg of sodium thiosulfate, 4.5 kg of hydroxypropyl methylcellulose, 25 kg of the antibacterial modifier prepared in Preparation Example 2 and 829 kg of water were stirred and mixed uniformly, and sealed to obtain the polycarboxylic acid water-reducing agent.
[0071] Example 3
[0072] This embodiment provides a polycarboxylate water-reducing agent, which is prepared by the following steps:
[0073] 80 kg of polycarboxylic acid water-reducing agent mother liquor, 50 kg of polycarboxylic acid collapse-preventing agent mother liquor, 12 kg of sodium tripolyphosphate, 12 kg of sodium gluconate, 18 kg of sodium thiosulfate, 6 kg of hydroxypropyl methylcellulose, 30 kg of the antibacterial modifier prepared in Preparation Example 3 and 792 kg of water were stirred and mixed uniformly, and sealed to obtain the polycarboxylic acid water-reducing agent.
[0074] Example 4
[0075] This embodiment provides a polycarboxylate water-reducing agent, which is different from Embodiment 2 in that:
[0076] The antibacterial modifier is prepared in Preparation Example 8.
[0077] Example 5
[0078] This embodiment provides a polycarboxylate water-reducing agent, which is different from Embodiment 2 in that:
[0079] The antibacterial modifier is prepared in Preparation Example 9.
[0080] Comparative Example
[0081] Comparative Example 1
[0082] This comparative example provides a polycarboxylate water-reducing agent, which is different from Example 2 in that:
[0083] The antibacterial modifier is prepared in Preparation Example 4.
[0084] Comparative Example 2
[0085] This comparative example provides a polycarboxylate water-reducing agent, which is different from Example 2 in that:
[0086] The antibacterial modifier is prepared in Preparation Example 5.
[0087] Comparative Example 3
[0088] This comparative example provides a polycarboxylate water-reducing agent, which is different from Example 2 in that:
[0089] The antibacterial modifier is prepared in Preparation Example 6.
[0090] Comparative Example 4
[0091] This comparative example provides a polycarboxylate water-reducing agent, which is different from Example 2 in that:
[0092] The antibacterial modifier is prepared in Preparation Example 7.
[0093] Comparative Example 5
[0094] This comparative example provides a polycarboxylic acid water-reducing agent, which is different from Example 2 in that the antibacterial modifier is hydrophilic nano-titanium dioxide.
[0095] Comparative Example 6
[0096] This comparative example provides a polycarboxylate water-reducing agent, which is different from Example 2 in that no antibacterial modifier is added.
[0097] Table 2 Examples and Preparation Examples Raw Materials (kg)
[0098]
[0099]
[0100] Performance Testing The examples or comparative examples were placed in an environment of 35° C. and 80% humidity, and the observations were recorded at 30, 60, 90 and 180 days respectively.
[0101] According to the following mix ratio, the polycarboxylate water-reducing agent prepared in the embodiment and the comparative example was mixed with other raw materials to prepare concrete, and then the working performance and compressive strength of the concrete were tested.
[0102] PO42.5R cement 200kg, S95 grade mineral powder 100kg, Ⅰ grade fly ash 80kg, fineness modulus 2.6 machine-made sand 770kg, 5-31.5mm continuous graded crushed stone 1060kg, water 160kg, water reducer 6.5kg. The water reducer is stored at 35℃ and 80% humidity for 180 days before use.
[0103] The slump of concrete is tested according to GB / T 50080-2016 "Standard for test methods for properties of ordinary concrete mixtures".
[0104] The 28d compressive strength of concrete is tested according to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".
[0105] Table 3 Performance test table
[0106]
[0107] It can be seen from Example 2, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5 and Table 3 that the antibacterial component is combined with the load component, and the overall stability of the antibacterial modifier is improved by the stabilizing component, so that the antibacterial performance of the prepared polycarboxylate water-reducer is effectively improved, thereby reducing the corruption and deterioration of the polycarboxylate water-reducer due to microbial reproduction, and reducing the adverse effects on product performance.
[0108] It can be seen from Example 2, Comparative Example 1, Comparative Example 3, Comparative Example 4 and Comparative Example 5 and Table 3 that the antibacterial modifier is prepared by mixing the antibacterial component with the stabilizing component using linear low-density polyethylene and polyethylene wax as loading components, thereby effectively improving the overall stability of the antibacterial modifier.
[0109] Combining Example 2, Example 4 and Example 5 with Table 3, it can be seen that after the antibacterial modifier is uniformly mixed with other raw materials, catechins and honeysuckle extract are permeated by water and dissolved in water, thereby improving the antibacterial performance of the polycarboxylate water reducer, while the inorganic antibacterial material continues to play an antibacterial role, further improving the antibacterial performance of the polycarboxylate water reducer.
[0110] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A polycarboxylate water reducer, characterized in that: The invention comprises 60 to 80 parts of a polycarboxylic acid water-reducing agent mother liquor, 30 to 50 parts of a polycarboxylic acid slump-retaining agent mother liquor, 24 to 48 parts of a functional material, 20 to 30 parts of an antibacterial modifier, and water is added to 1000 parts. The antibacterial modifier comprises an antibacterial component, a load component and a stabilizing component, and the weight ratio of the antibacterial component, the load component and the stabilizing component is 25:1 to 2:1 to 3. The antibacterial component comprises an organic antibacterial material and an inorganic antibacterial material, and the weight ratio of the organic antibacterial material to the inorganic antibacterial material is 1:1-3; The organic antibacterial material is catechin and honeysuckle extract, the weight ratio of the catechin and honeysuckle extract is 1:1, the inorganic antibacterial material is nano copper oxide and nano montmorillonite, the weight ratio of the nano copper oxide and nano montmorillonite is 1:1-5; The load component includes linear low-density polyethylene and polyethylene wax, and the weight ratio of the two is 19:1; The stabilizing component is hydrophilic nano titanium dioxide; The functional material comprises sodium tripolyphosphate, sodium gluconate, sodium thiosulfate and hydroxypropyl methylcellulose, and the weight ratio of the sodium tripolyphosphate, sodium gluconate, sodium thiosulfate and hydroxypropyl methylcellulose is 2:2:3:
1.
2. The method for preparing the polycarboxylate water-reducing agent according to claim 1, characterized in that: The method comprises the following steps: mixing a polycarboxylate water-reducing agent mother liquor, a polycarboxylate collapse-preventing agent mother liquor, a functional material and an antibacterial modifier, adding water to make up to 1000 parts, stirring and mixing evenly, and sealing to obtain the polycarboxylate water-reducing agent.
3. The method for preparing a polycarboxylate water-reducing agent according to claim 2, characterized in that: The preparation of the antibacterial modifier comprises the following steps: mixing the antibacterial component, the load component and the stabilizing component, preparing particles through melting, extrusion and granulation, and then freezing through liquid nitrogen and crushing, thereby preparing the antibacterial modifier.