A low temperature sintered high-medium rotation magnetic ferrite material and preparation method thereof

Through the co-substitution of Bi, Ti, Ca, V, Zr plasma and the doping of BBSZ glass and MoO3, the compatibility of gyromagnetic YIG ferrite materials in high dielectric constant, low ferromagnetic resonance line width and low-temperature sintering is solved problem, the optimization of dielectric constant and ferromagnetic resonance linewidth has been achieved, and the development of miniaturization and integration of gyromagnetic devices has been promoted.

CN116496080BActive Publication Date: 2024-10-08HUAYANG TECH DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310532107.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-10-08
Estimated Expiration
2043-05-11

Smart Images

  • Figure CN116496080B_ABST
    Figure CN116496080B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of electronic materials, and in particular to a low-temperature sintered high-medium-rotation magnetic ferrite material and a preparation method thereof. The low-temperature sintered high-medium-rotation magnetic ferrite material has a molecular formula of Bi 1.45 Ti 0.1 Y 1.55‑2x‑y Ca 2x+y V x Zr y‑0.1 Fe 5‑y‑x O 12 , wherein x is 0.6-0.65, y is 0.25-0.35, and 1.55-2x-y≥0. The preparation method provided by the present invention can not only realize low-temperature sintering at 900°C, but also realize good co-firing compatibility with the silver electrode of the LTCC process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic materials, and in particular to a low-temperature sintered high-medium-rotation magnetic ferrite material and a preparation method thereof. Background Art

[0002] Microwave gyromagnetic ferrite devices represented by circulators and isolators play a very important role in modern wireless communication systems. In recent years, with the rapid development of defense and civilian wireless communication technologies, the development trend of miniaturization, broadband and multi-function has become more and more obvious in various communication electronic products. Therefore, the microwave gyromagnetic devices widely used in them must also continue to develop in the direction of miniaturization and integration. Since the wavelength of electromagnetic waves propagating in the medium is inversely proportional to the square root of the dielectric constant, improving the dielectric constant of gyromagnetic ferrite materials has first become an important means to achieve the miniaturization of microwave ferrite devices.

[0003] LTCC (low temperature co-fired ceramic) technology can realize the three-dimensional structural design and packaging of passive electronic components, which is not only more conducive to the miniaturization and integration of electronic components, but also provides a new way for the innovative structural design of electronic components. Although LTCC technology has been widely used in many passive electronic components, it has hardly been involved in gyromagnetic devices. This is mainly because the sintering temperature of conventional gyromagnetic YIG ferrite materials is too high, and LTCC technology uses silver as a co-fired electrode material. If it is to be compatible with the LTCC process, the gyromagnetic material must be reduced to 900℃ or below for sintering density. The current commercially available low-linewidth gyromagnetic YIG ferrite materials generally have a dielectric constant of only 13 to 15, and the sintering temperature is as high as 1300 to 1450℃. Therefore, it is very difficult to simultaneously take into account the target requirements of high dielectric constant, low temperature sintering and low ferromagnetic resonance linewidth, and comprehensive innovative adjustments in material formulation and process are required.

[0004] In the research and development of high dielectric constant gyromagnetic YIG ferrite materials, the US invention patent (application number US13484018) first applied by Transtech in 2016 proposed that the use of appropriate amounts of Bi to replace Y can effectively improve the dielectric constant of gyromagnetic YIG materials, but the reported high dielectric constant gyromagnetic YIG ferromagnetic resonance line width is still relatively high (over 50Oe), and low-temperature sintering at 900°C or below has not been achieved. In the Chinese invention patent (publication number CN111285673A) applied by Shenzhen Sunlord Electronics Co., Ltd. in 2018, Bi, Ca, Zr, Al and Mn plasma co-replacement was used to improve the dielectric constant of the material, but the ferromagnetic resonance line width of the same material was also large (over 45Oe), and the material did not achieve low-temperature sintering. In 2021, Hengdian Group DMEGC Co., Ltd. also applied for a Chinese invention patent (publication number CN113896521A), which adopted a method of co-substitution of 10 elements including Bi, Gd, Ca, Nb, and V to achieve a low-linewidth, high-dielectric gyromagnetic ferrite material with a ferromagnetic resonance linewidth of about 20Oe and a dielectric constant of 25 to 28. However, this material only takes into account high dielectric constant and low linewidth, but the material system has not achieved low-temperature sintering. Combining all the relevant research reports at present, it can be found that there have been some research reports at home and abroad on improving the dielectric constant of gyromagnetic YIG materials, but there are currently no research reports on how to further achieve low-temperature sintering of high-dielectric gyromagnetic materials so that they can be combined with LTCC technology. Summary of the invention

[0005] In order to overcome the defects of the prior art, the technical problem to be solved by the present invention is to provide a gyromagnetic ferrite material having the characteristics of low temperature sintering, high dielectric constant and low ferromagnetic resonance line width and a preparation method thereof.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a low temperature sintered high-medium rotation magnetic ferrite material, the molecular formula of which is Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 , where x is 0.6~0.65, y is 0.25~0.35, and 1.55-2x-y≥0.

[0007] Another technical solution adopted by the present invention is: a method for preparing the above-mentioned low-temperature sintered high-medium rotation magnetic ferrite material, comprising the following steps:

[0008] S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 as initial raw materials, batching, mixing, ball milling, drying and pre-calcining are carried out in sequence according to the molecular formula of the gyromagnetic ferrite material to obtain a pre-calcined material;

[0009] S2: After the pre-sintered material is coarsely crushed, BBSZ (Bi2O3-H3BO3-SiO2-ZnO) glass and MoO3 are added, ball-milled again, and then dried to obtain a second dried material;

[0010] S3: The dried material is granulated, pressed and sintered in sequence to obtain a gyromagnetic ferrite material.

[0011] The beneficial effect of the present invention is that the present invention provides a high-dielectric and low-temperature sintered gyromagnetic material with 4πMs of about 780 to 830Gs, a dielectric constant of about 26.5 to 27.5, and a ferromagnetic resonance line width of ≤25Oe. The material well takes into account the comprehensive target requirements of suitable saturation magnetization intensity, high dielectric constant, low ferromagnetic resonance line width and 900°C low-temperature sintering, and is expected to well promote the combined development of LTCC technology and gyromagnetic devices, and be widely used in new small integrated LTCC gyromagnetic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 Shown is a process flow chart of a method for preparing a low temperature sintered high-medium rotation magnetic ferrite material in a specific embodiment of the present invention. DETAILED DESCRIPTION

[0013] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.

[0014] The key concept of the present invention is that the high-medium-magnetic ferrite material, the molecular formula of which is Bi 1.45 Ti 0.1 Y 1.55-2x- y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 It can not only achieve low-temperature sintering at 900°C, but also achieve good co-firing compatibility with the silver electrodes of the LTCC process.

[0015] The present invention discloses a low temperature sintered high mesotropic magnetic ferrite material, the molecular formula of which is Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O12 , where x is 0.6~0.65, y is 0.25~0.35, and 1.55-2x-y≥0.

[0016] From the above description, it can be seen that the beneficial effects of the present invention are: the low-temperature sintered high-rotation magnetic ferrite material of the present invention can finally achieve a performance of 4πMs of about 780 to 830Gs, a dielectric constant of about 26.5 to 27.5, and a ferromagnetic resonance line width of ≤25Oe. It can not only achieve low-temperature sintering at 900°C, but also achieve good co-firing compatibility with the silver electrodes of the LTCC process.

[0017] The formula of the present invention first adopts the co-substitution of Ca and V ions to obtain the required 4πMs, then improves the dielectric constant by replacing Bi ions appropriately, and finally further improves the dielectric constant by co-substitution of Ca and Ti ions, which has the following advantages:

[0018] (1) The substitution amount of Bi ions in the gyromagnetic ferrite is controlled at 1.45, which can maximize the comprehensive requirements of the material's high dielectric constant and low ferromagnetic resonance linewidth. At the same time, the sintering temperature of the material system is not too high, which is conducive to further reducing the sintering temperature to 900°C.

[0019] (2) The use of 0.1 mol of Ti ions for substitution is strictly controlled, which not only helps to improve the dielectric constant of the material system, but also can control the ferromagnetic resonance line width of the material not to be too high. The combination of Ti ions and Ca ions can satisfy the valence balance.

[0020] (3) The co-replacement method of Ca, V and Zr ions was adopted. On the one hand, the 4πMs of the material system can be controlled at about 780-830Gs by appropriate substitution amount, thus meeting the design requirements of low-field gyromagnetic devices; on the other hand, the sintering temperature of the material system can be further reduced by large-dose V ion substitution, which is more conducive to the low-temperature sintering of the material system. The appropriate substitution of Bi and V ions not only improves the dielectric constant and adjusts the 4πMs value, but also reduces the sintering temperature of the material system as much as possible; in addition, the appropriate amount of Ca and Zr ion substitution is also beneficial to reducing the ferromagnetic resonance linewidth of the material system.

[0021] Please refer to Figure 1 As shown, another technical solution adopted by the present invention is: a method for preparing the above-mentioned low-temperature sintered high-medium rotation magnetic ferrite material, comprising the following steps:

[0022] S1: Using Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 as initial raw materials, batching, mixing, ball milling, drying and pre-calcining are carried out in sequence according to the molecular formula of the gyromagnetic ferrite material to obtain a pre-calcined material;

[0023] S2: After the pre-sintered material is coarsely crushed, BBSZ glass and MoO3 are added, ball-milled again, and then dried to obtain a second dried material;

[0024] S3: The dried material is granulated, pressed and sintered in sequence to obtain a gyromagnetic ferrite material.

[0025] From the above description, it can be seen that the preparation method of the present invention first pre-fires the raw materials after the raw materials are divided into components and dried by ball milling once, and then doped with BBSZ glass and MoO3 in the pre-fired materials during the second ball milling. After the second ball milling and drying, PVA solution is added for granulation and molding, and finally sintering can achieve full densification to obtain a gyromagnetic ferrite material with low-temperature sintering, high dielectric constant and low ferromagnetic resonance line width characteristics. The material has been verified by co-firing with Ag powder, and no new phase is generated. It can not only achieve low-temperature sintering at 900°C, but also achieve good co-firing compatibility with the silver electrode of the LTCC process, and can be used for the research and development and application of LTCC gyromagnetic devices.

[0026] By doping an appropriate amount of BBSZ glass and MoO3 during the secondary ball milling, on the one hand, the sintering temperature of the material system can be reduced to 900°C through further liquid phase flux-assisted sintering to achieve low-temperature sintering compatible with the LTCC process and improve the density. Secondly, the material performance can be improved by optimizing the micromorphology of the ferrite material, which is beneficial to reducing the ferromagnetic resonance linewidth and improving the dielectric constant.

[0027] Furthermore, the pre-burning is specifically as follows: the dried material obtained after drying is sieved, compacted and punched, heated to 750-850° C. and kept warm for 6-8 hours for pre-burning, and the pre-burned material is obtained after cooling.

[0028] From the above description, it can be seen that during pre-sintering, the diffusion of ions and vacancies completes the solid phase reaction and grain growth, thereby improving the material properties.

[0029] Furthermore, the added amount of BBSZ glass is 0.2-0.3wt% of the weight of the pre-sintered material.

[0030] From the above description, we can see that

[0031] Furthermore, the weight ratio of BBSZ glass to MoO3 is 2 to 3:1.

[0032] From the above description, we can know that if the doping amount of BBSZ glass is too little, the material cannot be sufficiently densified at a low temperature of 900 degrees. If the doping amount of BBSZ glass is too much, the magnetic properties will decrease, which is typically reflected in the increase of the ferromagnetic resonance line width. Doping MoO3 helps to improve the microstructure of ferrite, make the grain growth more uniform, and increase the average grain size. 3的 Too little doping will not improve the microstructure, while too much doping will easily lead to uneven grain growth, which will in turn deteriorate the magnetic properties of the material.

[0033] From the above description, it can be seen that the combined doping mode of BBSZ glass + MoO3 used in the present invention can more effectively reduce the sintering temperature of the material system to 900° C., while the effect on the magnetic properties of the material is almost negligible.

[0034] Furthermore, the powder is ball-milled again until the average particle size is below 1 μm.

[0035] From the above description, it can be seen that the smaller the particles, the larger the specific surface area, and the greater the activity, which is beneficial to lowering the sintering temperature and reducing the reaction time.

[0036] Furthermore, the preparation method of BBSZ glass is as follows: weigh Bi2O3, H3BO3, SiO2 and ZnO raw materials, add deionized water to ball mill and mix evenly, then dry, then heat to 950-1050°C and keep warm for 1 hour, then pour into deionized water for rapid quenching, ball mill the glass slag obtained after rapid quenching to a particle size of 2-3um and then dry to obtain BBSZ glass.

[0037] Furthermore, during granulation, a PVA (polyvinyl alcohol) solution accounting for 8% to 12% of the weight of the re-dried material is added.

[0038] Furthermore, the specific steps during sintering are: heating to 150-200°C at 2-3°C / min, keeping warm for 1-2 hours, then draining the water; heating to 500-600°C at 2-3°C / min, keeping warm for 2-4 hours, then debinding; finally heating to 900°C at 2-3°C / min, keeping warm for 4-6 hours, and completing sintering after cooling.

[0039] From the above description, it can be seen that sintering allows the particles inside the material to interact with each other, eliminate pores, increase density, and complete solid-phase reaction.

[0040] Please refer to Figure 1 As shown, the first embodiment of the present invention is: a method for preparing a low temperature sintered high-medium rotation magnetic ferrite material, comprising the following steps:

[0041] S1: Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 with a purity of more than 99.5% are used as the initial raw materials. According to the molecular formula of the gyromagnetic ferrite material Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 The ingredients are accurately mixed, wherein x is 0.6-0.65, y is 0.25-0.35, and 1.55-2x-y≥0, and then mixed and ball-milled in a planetary ball mill for 6 hours and then dried.

[0042] S2. The dried material obtained after drying is passed through a 60-mesh sieve, compacted and punched, heated to 800° C. at a heating rate of 3° C. / min and kept warm for 6 hours for pre-burning, and cooled to room temperature with the furnace to obtain a pre-burned material.

[0043] S3: After the pre-sintered material is coarsely crushed, 0.25wt% of BBSZ glass and 0.1wt% of MoO3 are added to the pre-sintered material for trace doping; then, the pre-sintered material is ball-milled again in a planetary ball mill for 6h until the average particle size of the powder is less than 1μm, and then dried to obtain a second dried material;

[0044] The preparation method of BBSZ glass is as follows: Bi2O3, H3BO3, SiO2 and ZnO raw materials are weighed according to the molar fraction of 27% Bi2O3-35% H3BO3-6% SiO2-32% ZnO, deionized water is added for ball milling and mixing, and then the mixture is dried. The mixture is then heated to 1000°C and kept warm for 1 hour, and then poured into deionized water for rapid quenching. The glass slag obtained after rapid quenching is ball milled to a particle size of 2.5um and then dried to obtain BBSZ glass.

[0045] S4: Adding 10% of the weight of PVA solution to the dried material again and pressing and molding to obtain a green embryo.

[0046] S5: The green sample is heated to 200°C at 2°C / min and kept at this temperature for 2 hours, then the water is drained, then the temperature is heated to 600°C at 2°C / min and kept at this temperature for 3 hours, then the binder is drained, and finally the temperature is heated to 900°C at 2.5°C / min and kept at this temperature for 5 hours. The green sample is cooled to room temperature in the furnace and the sintering is completed to obtain the spin magnetic ferrite material.

[0047] Table 1 shows the test results obtained when x and y in the formula molecular formula take different values.

[0048] Table 1

[0049]

[0050] As can be seen from Table 1, the low-temperature sintered high-mesh ferrite material of the present invention can ultimately achieve a performance of 4πMs of about 780 to 830Gs, a dielectric constant of about 26.5 to 27.5, and a ferromagnetic resonance line width of ≤25Oe. It can not only achieve low-temperature sintering at 900°C, but also achieve good co-firing compatibility with the silver electrodes of the LTCC process.

[0051] Embodiment 2 of the present invention is: a method for preparing a low-temperature sintered high-medium-rotation ferrite material, comprising the following steps:

[0052] S1: Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 with a purity of more than 99.5% are used as the initial raw materials. According to the molecular formula of the gyromagnetic ferrite material Bi1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 The ingredients were precisely proportioned, where x=0.6, y=0.25, and then mixed and ball-milled in a planetary ball mill for 6 hours before drying.

[0053] S2. The dried material obtained after drying is passed through a 60-mesh sieve, compacted and punched, heated to 750° C. at a heating rate of 3° C. / min and kept warm for 8 hours for pre-burning, and cooled to room temperature with the furnace to obtain a pre-burned material.

[0054] S3: After the pre-sintered material is coarsely crushed, 0.2wt% of BBSZ glass and 0.1wt% of MoO3 are added to the pre-sintered material for trace doping; then the pre-sintered material is ball-milled again in a planetary ball mill for 6h until the average particle size of the powder is less than 1μm, and then dried to obtain a second dried material;

[0055] The preparation method of BBSZ glass is as follows: weigh Bi2O3, H3BO3, SiO2 and ZnO raw materials according to the molar fraction of 27% Bi2O3-35% H3BO3-6% SiO2-32% ZnO, add deionized water to ball-mill and mix evenly, then dry, then heat to 950°C and keep warm for 1 hour, then pour into deionized water for rapid quenching, ball-mill the glass slag obtained after rapid quenching to a particle size of 2um and then dry to obtain BBSZ glass.

[0056] S4: Add 8% PVA solution by weight to the dried material again and press it into shape to obtain a green embryo.

[0057] S5: The green embryo sample is heated to 150°C at 2.5°C / min and kept at this temperature for 1.8 hours, then the water is drained; the green embryo sample is heated to 500°C at 2.5°C / min and kept at this temperature for 4 hours, then the binder is drained; finally, the green embryo sample is heated to 900°C at 2°C / min and kept at this temperature for 4 hours, then the green embryo sample is cooled to room temperature in the furnace, and the sintering is completed to obtain the spin magnetic ferrite material.

[0058] Embodiment 3 of the present invention is: a method for preparing a low temperature sintered high-medium rotation magnetic ferrite material, comprising the following steps:

[0059] S1: Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 with a purity of more than 99.5% are used as the initial raw materials. According to the molecular formula of the gyromagnetic ferrite material Bi 1.45 Ti 0.1 Y 1.55-2x-y Ca 2x+y V x Zr y-0.1 Fe5-y-x O 12 The ingredients were accurately mixed, where xx=0.6, y=0.25, and then mixed and ball-milled in a planetary ball mill for 6 hours and then dried.

[0060] S2. The dried material obtained after drying is passed through a 60-mesh sieve, compacted and punched, heated to 850° C. at a heating rate of 3° C. / min and kept warm for 7 hours for pre-burning, and cooled to room temperature with the furnace to obtain a pre-burned material.

[0061] S3: After the pre-sintered material is coarsely crushed, 0.3wt% of BBSZ glass and 0.1wt% of MoO3 are added to the pre-sintered material for trace doping; then, the pre-sintered material is ball-milled again for 6h until the average particle size of the powder is less than 1μm, and then dried to obtain a second dried material;

[0062] The preparation method of BBSZ glass is as follows: Bi2O3, H3BO3, SiO2 and ZnO raw materials are weighed according to the molar fraction of 27% Bi2O3-35% H3BO3-6% SiO2-32% ZnO, deionized water is added to ball-mill and mix evenly, and then the mixture is dried. The mixture is then heated to 1050°C and kept warm for 1 hour, and then poured into deionized water for rapid quenching. The glass slag obtained after rapid quenching is ball-milled to a particle size of 3um and then dried to obtain BBSZ glass.

[0063] S4: Adding 12% of the weight of PVA solution to the dried material again and pressing and molding to obtain a green embryo.

[0064] S5: The green embryo sample is heated to 170°C at 3°C / min and kept at this temperature for 1 hour, then the water is drained, then the temperature is heated to 550°C at 3°C / min and kept at this temperature for 2 hours, then the binder is drained, and finally the temperature is heated to 900°C at 3°C / min and kept at this temperature for 6 hours. The green embryo sample is cooled to room temperature in the furnace to complete the sintering, and the gyromagnetic ferrite material is obtained.

[0065] In summary, the preparation method of the present invention provided by the present invention first pre-fires each raw material after being batched according to the components and dried by ball milling once, and doped with pre-fired BBSZ glass and MoO3 during the second ball milling, and after the second ball milling and drying, PVA solution is added for granulation and molding, and finally sintering can achieve full densification to obtain a gyromagnetic ferrite material with low-temperature sintering, high dielectric constant and low ferromagnetic resonance line width characteristics. The material adopts the substitution of suitable Bi and V ions to improve the dielectric constant, adjust the 4πMs value, and reduce the sintering temperature of the material system as much as possible, and then dopes an appropriate amount of BBSZ glass and MoO3 during the second ball milling, and the sintering temperature of the material system is further liquid phase flux sintering, and is reduced to 900°C to achieve low-temperature sintering compatible with the LTCC process and improve density. The material is verified by co-firing with Ag powder, and no new phase is generated. It can not only achieve 900°C low-temperature sintering, but also can achieve good co-firing compatibility with the silver electrode of the LTCC process, and can be used for the research and development application of LTCC gyromagnetic devices.

[0066] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a low temperature sintered high-medium rotation magnetic ferrite material, characterized in that: The following steps are involved: S1: Bi2O3, Y2O3, TiO2, CaCO3, V2O5, ZrO2 and Fe2O3 are used as initial raw materials, and the materials are batched, mixed, ball-milled, dried and pre-fired in sequence according to the molecular formula of the gyromagnetic ferrite material to obtain a pre-fired material; the molecular formula is Bi 1.45 Ti 0.1 Y 1.55-2x- y Ca 2x+y V x Zr y-0.1 Fe 5-y-x O 12 , where x is 0.6~0.65, y is 0.25~0.35, 1.55-2x-y≥0; S2: After the pre-sintered material is coarsely crushed, BBSZ glass and MoO3 are added, ball-milled again, and then dried to obtain a second dried material; S3: granulating, pressing and sintering the dried material again in sequence to obtain a gyromagnetic ferrite material; the specific steps of the sintering are: heating to 150-200°C at 2-3°C / min, keeping warm for 1-2 hours, then draining, then heating to 500-600°C at 2-3°C / min, keeping warm for 2-4 hours, then debinding, finally heating to 900°C at 2-3°C / min, keeping warm for 4-6 hours, and completing sintering after cooling; The added amount of the BBSZ glass is 0.2-0.3wt% of the weight of the pre-sintered material; the weight ratio of the BBSZ glass to MoO3 is 2-3:1; The preparation method of the BBSZ glass is as follows: weigh 27% Bi2O3, 35% H3BO3, 6% SiO2 and 32% ZnO raw materials in mole fraction, add deionized water to ball-mill and mix evenly, then dry, then heat to 950-1050°C and keep warm for 1 hour, then pour into deionized water for rapid quenching, ball-mill the glass slag obtained after rapid quenching to a particle size of 2-3um, and then dry to obtain BBSZ glass.

2. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 1, characterized in that: The pre-burning is specifically as follows: the dried material obtained after drying is sieved, compacted and punched, heated to 750-850° C. and kept warm for 6-8 hours for pre-burning, and the pre-burned material is obtained after cooling.

3. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 1, characterized in that: The ball milling is repeated until the average particle size of the powder is below 1 μm.

4. The method for preparing a low temperature sintered high-medium rotation magnetic ferrite material according to claim 1, characterized in that: During the granulation, a PVA solution accounting for 8% to 12% of the weight of the re-dried material is added.