Unfired pearlescent ceramic tile and preparation method thereof

By using electrostatic spraying technology to prepare γ-Ca2SiO4 and β-Ca2SiO4 powders and mica-titanium pearlescent pigments using industrial waste residue, combined with the carbonization reaction to form CaCO3 seed crystals, the problem of existing pearlescent ceramic glazes being easily decomposed at high temperatures has been solved and achieved The preparation of fire-free ceramic tiles with pearl luster effect has simple process, low cost and high adhesion, and is suitable for mass production.

CN116496107BInactive Publication Date: 2024-10-29HUBEI UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310472777.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing pearlescent ceramic glazes are easily decomposed at high temperatures, which limits their application in the ceramic industry. In addition, existing energy-saving and environmentally friendly preparation methods are costly, consume a lot of energy, and have limited types of pearlescent pigments, which cannot meet the artistic requirements of ceramics.

Method used

Industrial waste sugar filter mud and coal gangue are used to prepare γ-Ca2SiO4 and β-Ca2SiO4 powders. The mica titanium pearlescent pigment is adsorbed on the surface of the ceramic body through electrostatic spraying technology, and CaCO3 seeds are formed during the carbonization reaction to achieve the pearlescent effect. Preparation of no-fire ceramic tiles.

Benefits of technology

It realizes the preparation of ceramic tiles with simple process, low cost, short cycle and good pearl luster effect, avoids the high-temperature sintering process, has high bonding performance, is suitable for mass production, and meets the requirements of ceramic artistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116496107B_ABST
    Figure CN116496107B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramic tiles, and discloses a method for preparing unfired pearlescent ceramic tiles. Powder A and powder B are prepared by using industrial waste sugar filter mud, coal gangue and waste alkali residue. The main component of powder A is γ-Ca 2 SiO 4 , the main component of powder B is β-Ca 2 SiO 4 , after mixing powder A and powder B in a mass ratio of 4:1, spray them on the smooth and clean surface of the blank by electrostatic spraying. After compacting and polishing it, repeat the steps of electrostatic spraying to spray pearlescent pigment on the surface with a density of 1.5 g / cm 2 Then, the mixture was sprayed with softened water at a water-binder ratio of 1.5:1 and placed in a carbonization reactor, with CO introduced at a rate of 0.5 L / min. 2 Carry out carbonization curing reaction at normal pressure to obtain the unfired pearlescent ceramic tile. The present invention eliminates the high-temperature sintering process, avoids the decomposition of pearlescent pigments at high temperatures and the reaction with other components, obtains unfired pearlescent ceramic tiles with good adhesion, good pearl luster and artistic effect, and promotes the application of pearlescent pigments in the ceramic industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramics, and in particular relates to an unfired pearlescent ceramic tile prepared by utilizing industrial waste residues and a preparation method thereof. Background Art

[0002] Sugar filter mud is the industrial waste residue of the carbonate sugar factory. Its main component is calcium carbonate, but it contains some organic matter, which is very easy to mold and stink, causing water and air pollution. The main component of coal gangue is silicon dioxide, and it is also rich in metal oxides, alkaline earth metals and sulfides. It is a source of inorganic salt pollution and will pollute the environment through leaching of atmospheric precipitation. If these two types of industrial waste residues are reasonably utilized as resources, it will not only reduce environmental pollution, but also greatly reduce the cost of products, turning industrial waste residues into treasures.

[0003] Mica titanium pearlescent pigment is a kind of pearlescent pigment composed of mica coated with a thin layer of high-refractive metal oxides such as TiO2 and Fe2O3. It has been widely used in various fields. Adding pearlescent pigments to ceramic glazes can improve the brightness and glossiness of the glazes, and enhance the aesthetic value and artistic effect of ceramic products. Therefore, mica titanium pearlescent pigments are also widely used in the ceramic industry. However, pearlescent pigments are easily decomposed at high temperatures, so that they no longer have a pearlescent effect. They can only be used in low-temperature glazes, which limits the application of pearlescent pigments in the ceramic industry.

[0004] The patent application with publication number CN 107827363 A discloses a high-temperature golden pearlescent glaze and a preparation method. The method uses encapsulated high-temperature resistant pearlescent powder, frit powder and printing ink as raw materials, mixes them evenly, applies them to the surface of the ceramic body, screen prints them, and then burns them at a temperature of 1180~1230℃ after drying to obtain golden pearlescent glazed tiles. The glaze formula has a small number of raw materials, low cost, simple processing technology, and good bonding with the body or glaze. However, the encapsulated high-temperature resistant pearlescent requires additional packaging materials, has high production costs, and is easily affected by humidity. Therefore, this solution is not suitable for large-scale production of pearlescent ceramic glazes.

[0005] The patent application with publication number CN 111925121 A discloses an ultra-low temperature frit of non-melting pearlescent pigment and its preparation method. In this scheme, a certain mass of stone, kaolin, calcined alumina, silica fume, barium carbonate, carbonic acid, oxide and boric acid are used to prepare an ultra-low temperature frit glaze with a glaze firing temperature not higher than 1000°C, and non-melting pearlescent pigment is added thereto. The ultra-low temperature firing is carried out at a firing temperature of 650~750°C for 45~75 min, which can ensure that the pearlescent pigment in the glaze does not melt and obtain a good underglaze color or glaze color effect. However, this method requires secondary firing, has a high production cost, consumes a lot of energy, and cannot achieve true energy saving and environmental protection; and the types of non-melting pearlescent pigments are few, expensive, and have a large particle size. When used, the pearl luster effect is not obvious, which cannot meet people's requirements for ceramic artistry.

[0006] Different from the above patents, the ceramic tiles with pearl luster prepared by the present invention are attached to the ceramic body by carbonization. Because there is no high-temperature sintering process and the raw materials are simple, the decomposition of pearlescent pigments and reaction with other components at high temperatures are avoided, thereby preparing unfired ceramic tiles with good pearl luster effect. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a method for preparing a ceramic tile with pearl luster, which has the advantages of simple process, easy controllable operation, easy availability of raw materials, low cost and short cycle.

[0008] The specific steps of the technical solution are as follows:

[0009] A method for preparing an unfired pearl luster artistic glaze comprises the following steps:

[0010] 1) Pretreatment of raw materials: Place the sugar filter mud and coal gangue in a drying oven for 2-3 hours, crush and grind them separately, and then pass them through a 200-mesh sieve to obtain sugar filter mud powder and coal gangue powder.

[0011] 2) Weigh 40-55 parts of treated sugar filter mud and 15-20 parts of treated coal gangue powder, add water according to the solid-liquid mass ratio of (8-10):1, so that the calcium-silicon molar ratio in the raw materials is (2-2.5):1, mix well and press into sheets with a tablet press, sinter in a box furnace at 1320-1420 ℃, keep warm for 2 h, cool with the furnace and ball mill for 1-2 h to obtain powder A. Powder A is γ- Powder with Ca2SiO4 as the main component, including a small amount of Ca3SiO5, CaAl2O 4、 Ca3Al2O6, Ca4Fe2Al2O 10 , CaFeAlO4 and some aluminum silicates, etc.

[0012] 3) Weigh 35-45 parts of treated sugar filter mud, 15-20 parts of treated coal gangue powder and 1-2 parts of sintering aid, add water according to the solid-liquid mass ratio of (8-10):1, so that the calcium-silicon molar ratio in the raw materials is (2-2.5):1, mix well and press into sheets with a tablet press, sinter in a box furnace at 1320-1420 ℃, keep warm for 2 h, cool with the furnace and ball mill for 1-2 h to obtain powder B. Powder B is β -Ca2SiO4 powder as the main component, including a small amount of Ca3SiO5, CaAl2O 4、 Ca3Al2O6, Ca4Fe2Al2O 10 , CaFeAlO4 and some aluminum silicates, etc.

[0013] 4) Put the evenly milled powders A and B into the electrostatic spraying equipment, put the ceramic body into the spraying room, and bring the spraying equipment close to the ceramic body so that the powder is adsorbed on the surface of the body, apply pressure to make the powder and the body closely combined, and then grind it to make the surface smooth and flat.

[0014] 5) Put the pearlescent pigment into an electrostatic spraying device, put the green body obtained in step 5) into a spraying room, and place the spraying device close to the ceramic green body so that the pearlescent pigment is adsorbed on the surface of the green body.

[0015] 6) After spraying softened water on the surface of the green body with the material laid, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 to carry out a carbonization curing reaction. The carbonization time is 2 to 6 hours to obtain the unfired pearlescent ceramic tile.

[0016] Preferably, the sintering aid is waste alkali slag produced in Nanyang, Henan, the main components of which are 45 wt%~55 wt% Na2CO3 and 10 wt%~12 wt% NaCl.

[0017] Preferably, the mass ratio of powder A to powder B is (0.25~4):1.

[0018] Preferably, the pearlescent pigment is mica titanium pearlescent pigment, and the spraying density is 1.5 g / cm 2 . .

[0019] Preferably, the water-to-gel mass ratio is 1.5:1.

[0020] Preferably, in step 3), the ceramic glaze is applied to the bisque-fired body by dry electrostatic glazing, carbonized by atmospheric pressure, CO2 is introduced into the carbonization reactor at a rate of 0.5 L / min, and the carbonization time is 2 h to obtain the unfired ceramic tile with pearl luster.

[0021] The present invention uses industrial waste sugar filter mud, coal gangue and waste alkali residue to prepare γ- Ca2SiO4 and β -Ca2SiO4 is the main component of the powder, ball milled uniformly γ - Ca2SiO4 and β -Ca2SiO4 is electrostatically adsorbed onto the surface of the blank, and then 1.5 g / cm 2 Pearlescent pigment, after the material is laid, a layer of softened water is sprayed on the blank according to the water-binder ratio of 1.5:1, and it is placed in a carbonization reactor and CO2 is introduced for carbonization and curing reaction, and then carbonized at normal pressure to obtain a pearlescent unfired ceramic tile. 2+ from γ- Ca2SiO4 and β -Ca2SiO4 dissolves in the water. When CO2 is introduced, a surface effect is generated locally. 2+ When the two phases come into contact, the surface reaction begins, the temperature begins to rise, and CaCO3 seed crystals are rapidly generated at the interface. When the seed crystals begin to grow, the pearlescent pigments continue to accumulate and embed in the gaps between the crystals, and begin to increase in the vertical direction. As the most stable calcite crystal form among the CaCO3 crystal forms, the pearlescent pigments will be firmly attached to the gaps between the grains. Therefore, the glaze can be firmly attached to the ceramic body, thus achieving unfired ceramic tiles with pearl luster.

[0022] Compared with the prior art, the present invention has the following advantages and significant progress:

[0023] 1) This invention uses industrial waste sugar filter mud, coal gangue and waste alkali residue to prepare γ- Ca2SiO4 and β -The main powder of Ca2SiO4 and a small amount of Ca3SiO5, CaAl2O4 and CaFeAlO4. CaFeAlO4 and CaAl2O4 can solidify quickly, so the pearlescent pigment can be initially fixed on the ceramic body. After carbonization, CaCO3 seeds will be generated at the interface of the glaze and the body. At this time, the pearlescent pigment will continue to be enriched and embedded in the gaps between the crystals.

[0024] 2) The calcination temperature of mica titanium pearlescent pigment cannot exceed 800°C. When the temperature is too high, TiO2 and Fe2O3 in the mica titanium pearlescent pigment will react with oxides such as PbO and CaO in the base glaze, thereby deteriorating the pearlescent effect. The firing temperature of the glaze is basically around 1100°C. The present invention selects the CaCO3 phase of the calcite crystal formed by the carbonization of Ca2SiO4 at normal pressure as a binder to bond the ceramic body and the pearlescent pigment, thereby preparing unfired pearlescent ceramic tiles with good artistic effect and high bonding performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 XRD pattern of powder A

[0026] Figure 2 XRD pattern of powder B DETAILED DESCRIPTION

[0027] The technical scheme of the present invention is further specifically described below through examples, wherein powder A is γ- Powder with Ca2SiO4 as the main component, including a small amount of Ca3SiO5, CaAl2O 4、 Ca3Al2O6, Ca4Fe2Al2O 10 , CaFeAlO4 and some aluminum silicates, etc.; Powder B is based on β -Ca2SiO4 powder as the main component, including a small amount of Ca3SiO5, CaAl2O 4、 Ca3Al2O6, Ca4Fe2Al2O 10 , CaFeAlO4 and some aluminum silicates, etc.

[0028] Example 1

[0029] Step 1): Place 10 g of powder A that has been evenly ball-milled into an electrostatic spraying device, place a ceramic body in a spraying chamber, and place the spraying device close to the ceramic body so that the powder is adsorbed on the surface of the body, apply pressure to it so that the powder and the body are tightly combined, and then polish it to make the surface smooth and flat.

[0030] Step 2): Place the pearlescent pigment in the electrostatic spraying equipment, place the green body obtained in step 1) in the spraying room, and place the spraying equipment close to the ceramic green body so that the pearlescent pigment is adsorbed on the green body surface with a density of 1.5g / cm 2 .

[0031] Step 3): After spraying softened water on the surface of the body with the material laid according to a water-binder ratio of 1.5:1, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 for carbonization and curing reaction. The carbonization time is 2 hours to obtain the unfired pearlescent ceramic tile.

[0032] Example 2

[0033] Step 1): Put 8 g of ball-milled powder and 2 g of powder B into the electrostatic spraying equipment, put the ceramic body into the spraying room, and bring the spraying equipment close to the ceramic body so that the powder is adsorbed on the surface of the body, apply pressure to make the powder and the body tightly combined, and then polish it to make the surface smooth and flat.

[0034] Step 2): Place the pearlescent pigment in the electrostatic spraying equipment, place the green body obtained in step 1) in the spraying room, and place the spraying equipment close to the ceramic green body so that the pearlescent pigment is adsorbed on the green body surface with a density of 1.5g / cm 2 .

[0035] Step 3): After spraying softened water on the surface of the body with the material laid according to a water-binder ratio of 1.5:1, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 for carbonization and curing reaction. The carbonization time is 2 hours to obtain the unfired pearlescent ceramic tile.

[0036] Example 3

[0037] Step 1): Put 6 g of powder A and 4 g of powder B that have been evenly ball-milled into an electrostatic spraying device, put the ceramic body into the spraying room, and place the spraying device close to the ceramic body so that the powder is adsorbed on the surface of the body, apply pressure to it so that the powder and the body are tightly combined, and then polish it to make the surface smooth and flat.

[0038] Step 2): Place the pearlescent pigment in the electrostatic spraying equipment, place the green body obtained in step 1) in the spraying room, and place the spraying equipment close to the ceramic green body so that the pearlescent pigment is adsorbed on the green body surface with a density of 1.5g / cm 2 .

[0039] Step 3): After spraying softened water on the surface of the body with the material laid according to a water-binder ratio of 1.5:1, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 for carbonization and curing reaction. The carbonization time is 3 hours to obtain the unfired pearlescent ceramic tile.

[0040] Example 4

[0041] Step 1): Put 4 g of powder A and 6 g of powder B that have been evenly ball-milled into an electrostatic spraying device, put the ceramic body into the spraying room, and place the spraying device close to the ceramic body so that the powder is adsorbed on the surface of the body, apply pressure to it so that the powder and the body are tightly combined, and then polish it to make the surface smooth and flat.

[0042] Step 2): Place the pearlescent pigment in the electrostatic spraying equipment, place the green body obtained in step 1) in the spraying room, and place the spraying equipment close to the ceramic green body so that the pearlescent pigment is adsorbed on the green body surface with a density of 1.5g / cm 2 .

[0043] Step 3): After spraying softened water on the surface of the body with the material laid according to a water-binder ratio of 1.5:1, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 for carbonization and curing reaction. The carbonization time is 4 hours to obtain the unfired pearlescent ceramic tile.

[0044] Example 5

[0045] Step 1): Put 2 g of powder A and 8 g of powder B that have been evenly ball-milled into an electrostatic spraying device, put the ceramic body into the spraying room, and place the spraying device close to the ceramic body so that the powder is adsorbed on the surface of the body, apply pressure to it so that the powder and the body are tightly combined, and then polish it to make the surface smooth and flat.

[0046] Step 2): Place the pearlescent pigment in the electrostatic spraying equipment, place the green body obtained in step 1) in the spraying room, and place the spraying equipment close to the ceramic green body so that the pearlescent pigment is adsorbed on the green body surface with a density of 1.5g / cm 2 .

[0047] Step 3): After spraying softened water on the surface of the body with the material laid according to a water-binder ratio of 1.5:1, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 for carbonization and curing reaction. The carbonization time is 5 hours to obtain the unfired pearlescent ceramic tile.

[0048] Example 6

[0049] Step 1): Place 10g of powder B that has been evenly ball-milled into an electrostatic spraying device, place a ceramic body in a spraying room, and place the spraying device close to the ceramic body so that the powder is adsorbed on the surface of the body, apply pressure to it so that the powder and the body are tightly combined, and then polish it to make the surface smooth and flat.

[0050] Step 2): Place the pearlescent pigment in the electrostatic spraying equipment, place the green body obtained in step 1) in the spraying room, and place the spraying equipment close to the ceramic green body so that the pearlescent pigment is adsorbed on the green body surface with a density of 1.5g / cm 2 .

[0051] Step 3): After spraying softened water on the surface of the body with the material laid according to a water-binder ratio of 1.5:1, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 for carbonization and curing reaction. The carbonization time is 6 hours to obtain the unfired pearlescent ceramic tile.

[0052] Performance Test:

[0053] In order to test the adhesion of the pearlescent glaze on the ceramic tile, the present invention adopts the American standard test method for measuring adhesion by tape test (D3359-08) to test six samples of Examples 1 to 6.

[0054] The test steps are as follows: 2Cut a 5×5mm grid in the test area with a knife, place the center of the tape over the grid, and smooth the center of the grid into place with your fingers. Then, after 90±30 s, grab the free end, tear off the tape, and tear it off quickly (without shaking) at an angle as close to 180° as possible. Finally, use a magnifying glass to check the test area and determine the proportion of material drop by comparing it with the material attachment area before the test. The entire experiment was repeated three times. The test results are as follows:

[0055] Serial number First material drop ratio (%) Second material drop ratio (%) The third material drop ratio (%) Evaluation results Example 1 5 10 3 3B Example 2 0 0 0 5B Example 3 1 0 1 4B Example 4 0 1 1 4B Example 5 5 5 10 3B Example 6 3 2 6 3B

[0056] As can be seen from the above table, the pearlescent unfired ceramic tile of the present invention has excellent performance required by the market. Combining the above tests, it can be clearly seen that the excellent performance of the present invention is not only simple in preparation process, good in controllability, low in production cost, simple in raw materials, but also good in adhesion, high in artistic value, simple in process conditions and easy to repeat, and suitable for mass production.

Claims

1. A method for preparing unfired pearlescent ceramic tiles, characterized in that: The steps include: 1) Pretreatment of raw materials: Place the sugar filter mud and coal gangue in a drying oven for 2-3 hours, crush and grind them separately, and then pass them through a 200-mesh sieve to obtain sugar filter mud powder and coal gangue powder; 2) Weigh 40-55 parts of treated sugar filter mud and 15-20 parts of treated coal gangue powder, add water according to the solid-liquid mass ratio of (8-10):1, so that the calcium-silicon molar ratio in the raw materials is (2-2.5):1, mix well and press into sheets with a tablet press, sinter in a box furnace at 1320-1420 ℃, keep warm for 2 h, cool with the furnace and ball mill for 1-2 h to obtain powder A. Powder A is γ- Powder with Ca2SiO4 as the main component, including a small amount of Ca3SiO5, CaAl2O 4、 Ca3Al2O6, Ca4Fe2Al2O 10 , CaFeAlO4 and some aluminosilicates; 3) Weigh 35-45 parts of treated sugar filter mud, 15-20 parts of treated coal gangue powder and 1-2 parts of sintering aid, add water according to the solid-liquid mass ratio of (8-10):1, so that the calcium-silicon molar ratio in the raw materials is (2-2.5):1, mix well and press into sheets with a tablet press, sinter in a box furnace at 1320-1420 ℃, keep warm for 2 h, cool with the furnace and ball mill for 1-2 h to obtain powder B. Powder B is β -Ca2SiO4 powder as the main component, including a small amount of Ca3SiO5, CaAl2O 4、 Ca3Al2O6, Ca4Fe2Al2O 10 , CaFeAlO4 and some aluminosilicates; the sintering aid is waste alkali slag produced in Nanyang, Henan, the main components of which are 45 wt%~55wt% Na2CO3 and 10 wt%~12 wt% NaCl; 4) Put the evenly milled powders A and B into the electrostatic spraying equipment, put the ceramic body into the spraying room, and bring the spraying equipment close to the ceramic body so that the powders are adsorbed on the surface of the body; 5) placing the pearlescent pigment into an electrostatic spraying device, placing the green body obtained in step 4) into a spraying room, and placing the spraying device close to the ceramic green body so that the pearlescent pigment is adsorbed on the green body surface; 6) After spraying softened water on the surface of the green body with the material laid, place it in a vacuum drying oven for 15 minutes, and then put it into a carbonization reactor and introduce CO2 to carry out a carbonization curing reaction. The carbonization time is 2 to 6 hours to obtain the unfired pearlescent ceramic tile.

2. The preparation method according to claim 1, characterized in that: The sugar filter mud described in step 1) is industrial solid waste from a carbonate sugar factory, and its main components are 80 wt% to 85 wt% calcium carbonate, 5 wt% to 7 wt% crude protein and 8 wt% to 9 wt% sugar.

3. The preparation method according to claim 1, characterized in that: The coal gangue described in step 1) is solid waste discharged during coal mining and coal washing, and its main components are 55 wt%~70 wt% SiO2, 16 wt%~25 wt% Al2O3, 2 wt%~7wt% Fe2O3 and 0.4 wt%~2.5 wt% CaO.

4. The preparation method according to claim 1, characterized in that: Step 4) The powder was ball-milled for 1.5 hours and then passed through a 325 mesh.

5. The preparation method according to claim 1, characterized in that: The mass ratio of powder A to powder B is (0.25~4):

1.

6. The preparation method according to claim 1, characterized in that: In step 5), the pearlescent pigment is mica titanium pearlescent pigment, and the spraying density is 1.5-2 g / cm 2 .

7. The preparation method according to claim 1, characterized in that: Step 6) The softened water treatment process is an ion exchange method using a cation exchange resin for a treatment time of 10 to 15 minutes.

8. A fired pearlescent ceramic tile, characterized in that: The preparation method is described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • High-temperature golden yellow pearl glaze and application thereof

    CN107827363A

  • Ultralow-temperature frit of non-melting pearlescent pigment, preparation method of ultralow-temperature frit and ceramic glaze

    CN111925121A

  • Interference-effect enhanced pearlescent pigment preparation method and product thereof

    CN102876090A

  • Fiber cement board based on carbon dioxide driven consolidation and preparation method of fiber cement board

    CN113816668A