A composite catalyst and its preparation method and application

Through the coupling of modified iron-based metal oxides and HZSM-5 molecular sieve, the problems of low conversion and high selectivity in the carbon dioxide aromatic hydrocarbon catalyst are solved, and efficient aromatic hydrocarbon production is achieved, and the activity of the catalyst and aromatic hydrocarbon selectivity are improved.

CN116510770BActive Publication Date: 2024-11-12EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310083051.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2024-11-12
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

The existing carbon dioxide aromatic hydrocarbon catalysts have problems such as low carbon dioxide conversion, high selectivity of carbon monoxide and methane, and low yield of aromatic hydrocarbon products.

Method used

Modified iron-based metal oxide is used to couple it with HZSM-5 molecular sieve. By adjusting the molar ratio of zinc to iron and adding metal additives such as sodium, potassium, zinc, manganese, and copper, combined with polyethylene glycol structural additives, the catalyst is improved. activity and selectivity.

Benefits of technology

It significantly improves the conversion of carbon dioxide, reduces the selectivity of carbon monoxide and methane, improves the selectivity of aromatic hydrocarbons in total hydrocarbons, and achieves an efficient direct aromatic hydrocarbon production process of carbon dioxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116510770B_ABST
    Figure CN116510770B_ABST
Patent Text Reader

Abstract

The present application discloses a composite catalyst and its preparation method and application. The composite catalyst of the present application includes a modified iron-based metal oxide and a HZSM-5 molecular sieve; in the modified iron-based metal oxide, the molar ratio of zinc to iron is 1: (0-8); the modified iron-based metal oxide includes a metal additive, and the metal additive includes at least one element of sodium, potassium, zinc, manganese, and copper; the mass percentage of the metal additive in the composite catalyst is 0.5% to 8%. The composite catalyst of the present application solves the problems of low carbon dioxide conversion rate, high total selectivity of carbon monoxide and methane, and low yield of aromatic products in existing catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of catalyst technology, and in particular to a composite catalyst and a preparation method and application thereof. Background Art

[0002] As an important basic raw material in the chemical industry, aromatics are widely used in polymer synthetic materials, organic synthesis, fine chemical synthesis, organic solvents, pesticides, explosives, military industry, etc. In recent years, the technology of producing aromatics from carbon dioxide has become the focus of attention at home and abroad. Compared with the existing aromatics preparation technology, the technology of producing aromatics from carbon dioxide has cheaper and more available raw materials, which is more economically reasonable. On the other hand, this technology breaks the pattern that traditional aromatics production mainly relies on petroleum catalytic reforming, hydrocracking and coal-to-syngas to produce aromatics, which alleviates the shortage of fossil fuels. In addition, using carbon dioxide as a raw material for producing aromatics can greatly reduce carbon dioxide emissions.

[0003] In the prior art, the composite catalyst used in the preparation of aromatics from carbon dioxide has the disadvantages of low carbon dioxide conversion rate and high selectivity of byproduct carbon monoxide, resulting in low aromatic yield. In order to solve this problem, different research and development teams have modified composite catalysts to improve catalyst conversion rate and selectivity, but the selectivity of carbon monoxide is still very high, and the conversion rate of carbon dioxide also has room for improvement. Therefore, developing a carbon dioxide hydrogenation catalyst for direct preparation of aromatics that efficiently converts carbon dioxide is a technical difficulty that needs to be solved urgently.

[0004] Chinese patent CN115155588A discloses a tandem catalyst for preparing aromatic hydrocarbons by direct hydrogenation of carbon dioxide based on a modified Fischer-Tropsch synthesis route. xThe two parts are obtained by physical mixing, and the CO2 conversion rate is as high as 43.95%, and the aromatic selectivity can reach 39.79%. Although the CO2 conversion rate achieved by the catalyst used in this patent is high, the high aromatic selectivity is not obtained, resulting in a low total aromatic yield. Chinese patent CN109942359A discloses a composite double-bed catalyst, the first bed is composed of three-dimensional honeycomb graphene loaded with iron and potassium active components as a carrier, catalyzing the hydrogenation of carbon dioxide to generate intermediate products of light olefins; the second bed is composed of molecular sieves, and the light olefins produced by the first bed are subjected to aromatization reaction to generate aromatic products. The catalyst can achieve flexible regulation of aromatic composition while obtaining high aromatic selectivity, but its CO2 conversion rate is low. Chinese patent CN108160104A discloses a catalyst for the one-step hydrogenation of carbon dioxide to produce aromatics, which is composed of two parts: nano-scale metal oxide and HZSM-5 molecular sieve, wherein modified or unmodified Fe2O3 is used as the metal oxide. This catalyst can achieve higher aromatics selectivity and has the advantages of stable catalytic performance and long life, but its disadvantage is that it has high selectivity for carbon monoxide and low-carbon alkanes. Summary of the invention

[0005] The purpose of the present application is to provide a composite catalyst and its preparation method and application. The composite catalyst of the present application solves the problems of low carbon dioxide conversion rate, high total selectivity of carbon monoxide and methane, and low yield of aromatic products existing in the existing catalysts by modifying the iron-based metal oxide and coupling with HZSM-5 molecular sieve.

[0006] In a first aspect, an embodiment of the present application provides a composite catalyst, wherein the composite catalyst comprises a modified iron-based metal oxide and a HZSM-5 molecular sieve;

[0007] In the modified iron-based metal oxide, the molar ratio of zinc to iron is 1:(0-8); the modified iron-based metal oxide includes a metal additive, and the metal additive includes at least one element selected from the group consisting of sodium, potassium, zinc, manganese, and copper; the mass percentage of the metal additive in the composite catalyst is 0.5%-8%.

[0008] In some embodiments, the HZSM-5 molecular sieve includes a structural additive, and the mass percentage of the structural additive to the HZSM-5 molecular sieve is 1-2%; the structural additive includes polyethylene glycol.

[0009] In some embodiments, the pore volume of the HZSM-5 molecular sieve is 0.1 to 60 cm 3 / g, specific surface area is 150~500m 2 / g, the average pore size is 5-100nm, and the silicon-aluminum ratio is 20-150.

[0010] In some embodiments, the pore volume of the modified iron-based metal oxide is 0.10 to 0.45 cm 3 / g, specific surface area is 15~50m 2 / g, pore size is 10~60nm.

[0011] In some embodiments, the mass ratio of the modified iron-based metal oxide to the HZSM-5 molecular sieve is 1:(0.5-2).

[0012] In a second aspect, the embodiments of the present application further provide a method for preparing the composite catalyst, comprising the following steps:

[0013] Preparation of modified iron-based metal oxide: at a temperature of 50-70° C., an alkaline precipitant is added dropwise to a solution of iron nitrate and zinc nitrate in a molar ratio of 1:(0-8), and when the pH reaches 3.2-12, the titration end point is reached, and the solution is aged for 0.5-5 hours. After the aging is completed, the obtained reaction product is filtered, washed, and dried; the dried reaction product is calcined at 300-550° C. for 4-8 hours to obtain an iron-based metal oxide, the iron-based metal oxide is loaded with a metal additive by an impregnation method, the obtained product is dried, and calcined at 300-550° C. for 4-8 hours to obtain a modified iron-based metal oxide;

[0014] Preparation of HZSM-5 molecular sieve: tetraethyl orthosilicate, tetrapropylammonium hydroxide and polyethylene glycol in a molar ratio of 2: (0.01-2): (0-0.01) are mixed with deionized water to prepare a molecular sieve silicon source precursor solution, sodium aluminate is added to the molecular sieve silicon source precursor solution to obtain a suspension, the suspension is subjected to hydrothermal crystallization for 12-72 hours, the crystallization temperature is controlled at 100-180° C., the product obtained after the crystallization is completed is centrifuged and washed until the pH is neutral, dried and calcined, the calcination time is 2-8 hours, and the calcination temperature is 400-600° C. to obtain a Na-type ZSM-5 molecular sieve; the Na-type ZSM-5 molecular sieve is poured into an NH4Cl solution and stirred, the temperature is controlled at 50-100° C., ion exchange is performed for 2-4 hours, and then centrifuged and washed and dried, and calcined at 400-600° C. for 2-8 hours to obtain a HZSM-5 molecular sieve;

[0015] The iron-based metal oxide and the HZSM-5 molecular sieve are mixed to obtain a composite catalyst.

[0016] In some embodiments, the iron-based metal oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:(0.5-2) to obtain a composite catalyst.

[0017] In a third aspect, the embodiments of the present application further provide the use of the above-mentioned composite catalyst in the preparation of aromatics by hydrogenation of carbon dioxide.

[0018] In some embodiments, the above application includes the following steps: loading the composite catalyst into a reactor, introducing reducing gas hydrogen for reduction, and after the reduction is completed, introducing a reaction raw gas, wherein the volume ratio of H2 to CO2 in the reaction raw gas is 3 to 9, the reaction temperature is 280 to 380°C, and the reaction pressure is 2.6 to 4MPa.

[0019] In some embodiments, the space velocity of the reaction raw material gas is 500 to 6000 h -1 The reaction time is 24 to 72 hours.

[0020] The beneficial effects of the present application are as follows: the composite catalyst of the present application comprises a modified iron-based metal oxide and a HZSM-5 molecular sieve; in the modified iron-based metal oxide, the molar ratio of zinc to iron is 1:(0-8); the modified iron-based metal oxide comprises a metal additive, and the metal additive comprises at least one element of sodium, potassium, zinc, manganese, and copper; the mass percentage of the metal additive in the composite catalyst is 0.5%-8%. The composite catalyst of the present application is formed by mixing the modified iron-based metal oxide and the HZSM-5 molecular sieve in a mass ratio of 1:(0.5-2), which solves the problems of low carbon dioxide conversion rate, high total selectivity of carbon monoxide and methane, and low yield of aromatic products in the existing catalyst, and improves the carbon dioxide conversion rate and aromatic selectivity. The composite catalyst of the present application realizes efficient coupling of multi-step reactions in the process of direct production of aromatics by hydrogenation of carbon dioxide, and enhances the catalytic activity and service life of the composite catalyst, so that the reaction proceeds in a direction that is favorable to the target product. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0022] Figure 1 This application discloses a composite catalyst of modified iron-based metal oxide and HZSM-5 molecular sieve containing different iron-zinc metal ratios for the catalytic performance of directly producing high value-added aromatics from carbon dioxide. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application. In addition, in the description of the present application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as markings, and no numerical requirements or order are imposed. Various embodiments of the present application may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity, and should not be understood as a hard limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values ​​within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered range, such as 1, 2, 3, 4, 5 and 6, which are applicable regardless of the range. Additionally, whenever a numerical range is indicated herein, it is meant to include any cited numeral (fractional or integral) within the indicated range.

[0024] In order to solve the problems of low carbon dioxide conversion rate, high total selectivity of carbon monoxide and methane, and low yield of aromatic products in the prior art, the embodiment of the present application provides a composite catalyst, which includes a modified iron-based metal oxide and a HZSM-5 molecular sieve; in the modified iron-based metal oxide, the molar ratio of zinc to iron is 1: (0-8); the modified iron-based metal oxide includes a metal additive, and the metal additive includes at least one element of sodium, potassium, zinc, manganese, and copper; the mass percentage of the metal additive in the composite catalyst is 0.5% to 8%. The present application increases the carbon dioxide conversion rate and reduces the selectivity of CO by modifying the iron-based metal oxide.

[0025] In some embodiments, in the composite catalyst, the molar ratio of zinc to iron is any value of 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, or a range consisting of any two values.

[0026] When the modified iron-based metal oxide of the present invention is an iron-zinc bimetallic oxide catalyst, the carbon dioxide conversion rate can be increased, the selectivity of CO and methane can be reduced, and the product distribution can be adjusted to increase C 5+ The selectivity of total hydrocarbons and the selectivity of aromatic hydrocarbons in total hydrocarbons are improved.

[0027] The composite catalyst of the present application can directly produce aromatics in one step through carbon dioxide, avoiding a multi-step series of operations, and can minimize the number of devices and thus reduce the investment cost of device equipment, simplify the operation process, and reduce energy consumption in the production process.

[0028] The carbon dioxide conversion rate of the composite catalyst of the present application can reach up to 42.60%, the sum of carbon monoxide and methane selectivities can be limited to less than 15%, the liquid product selectivity can reach up to more than 70%, and the aromatics selectivity can reach up to 63.68%.

[0029] In some embodiments, the HZSM-5 molecular sieve includes a structural additive, and the mass percentage of the structural additive in the HZSM-5 molecular sieve is 1-2%; the structural additive includes polyethylene glycol.

[0030] In some embodiments, the mass percentage (%) of the structural additive to the HZSM-5 molecular sieve is: any value of 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, or a range consisting of any two values.

[0031] The composite catalyst of the present invention is added with a structural additive to further increase the C 5+ The selectivity for aromatics in total hydrocarbons is also improved, and the catalyst has good aromatic selectivity.

[0032] In some embodiments, the pore volume of the HZSM-5 molecular sieve is 0.1 to 60 cm 3 / g, specific surface area is 150~500m 2 / g, the average pore size is 5-100nm, and the silicon-aluminum ratio is 20-150.

[0033] In some embodiments, the pore volume (cm 3 / g) is any value of 0.1, 0.326, 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, or a range consisting of any two values.

[0034] In some embodiments, the specific surface area (m 2 / g) is any value of 150, 200, 250, 300, 322, 350, 400, 450, 500, or a range consisting of any two values.

[0035] In some embodiments, the average pore size (nm) of the HZSM-5 molecular sieve is any value of 5, 6.15, 10, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100, or a range consisting of any two values.

[0036] In some embodiments, the silicon-to-aluminum ratio of the HZSM-5 molecular sieve is any value of 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, or a range consisting of any two values.

[0037] In some embodiments, the pore volume of the modified iron-based metal oxide is 0.10 to 0.45 cm 3 / g, specific surface area is 15~50m 2 / g, pore size is 10~60nm.

[0038] In some embodiments, the pore volume (cm 3 / g) is any value among 0.10, 0.20, 0.2021, 0.2326, 0.25, 0.2538, 0.2836, 0.2964, 0.30, 0.35, 0.40, 0.45, or a range consisting of any two values.

[0039] In some embodiments, the specific surface area (m 2 / g) is any value of 15, 18.2561, 20, 23.2631, 25, 30, 31.2328, 33.2834, 35, 39.8431, 40, 45, 50, or a range consisting of any two values.

[0040] In some embodiments, the pore size (nm) of the modified iron-based metal oxide is any value of 10, 14.3567, 15, 17.6385, 20, 25, 26.2354, 30, 31.2321, 35, 40, 41.5163, 45, 50, 55, 60, or a range consisting of any two values.

[0041] In some embodiments, the mass ratio of the modified iron-based metal oxide to the HZSM-5 molecular sieve is 1:(0.5-2).

[0042] In some embodiments, the mass ratio of the modified iron-based metal oxide to the HZSM-5 molecular sieve is any value of 1:0.5, 1:1, 1:1.5, 1:2, or a range consisting of any two values.

[0043] In a second aspect, the embodiments of the present application further provide a method for preparing the composite catalyst, comprising the following steps:

[0044] Preparation of modified iron-based metal oxide: at a temperature of 50-70° C., an alkaline precipitant is added dropwise to a solution of iron nitrate and zinc nitrate in a molar ratio of 1:(0-8), and when the pH reaches 3.2-12, the titration end point is reached, and the solution is aged for 0.5-5 hours. After the aging is completed, the obtained reaction product is filtered, washed, and dried; the dried reaction product is calcined at 300-550° C. for 4-8 hours to obtain an iron-based metal oxide, the iron-based metal oxide is loaded with a metal additive by an impregnation method, the obtained product is dried, and calcined at 300-550° C. for 4-8 hours to obtain a modified iron-based metal oxide;

[0045] Preparation of HZSM-5 molecular sieve: tetraethyl orthosilicate, tetrapropylammonium hydroxide and polyethylene glycol in a molar ratio of 2: (0.01-2): (0-0.01) are mixed with deionized water to prepare a molecular sieve silicon source precursor solution, sodium aluminate is added to the molecular sieve silicon source precursor solution to obtain a suspension, the suspension is hydrothermally crystallized for 12-72 hours, the crystallization temperature is controlled at 100-180° C., the product obtained after the crystallization is completed is centrifugally washed until the pH is neutral, dried and calcined, the calcination time is 2-8 hours, and the calcination temperature is 400-600° C. to obtain a Na-type ZSM-5 molecular sieve; the Na-type ZSM-5 molecular sieve is poured into an NH4Cl solution and stirred, the temperature is controlled at 50-100° C., ion exchange is performed for 2-4 hours, and then centrifugally washed and dried, and calcined at 400-600° C. for 2-8 hours to obtain a HZSM-5 molecular sieve.

[0046] The iron-based metal oxide and the HZSM-5 molecular sieve are mixed to obtain a composite catalyst.

[0047] The composite catalyst preparation method of the present application is simple and easy to operate, the required raw materials are cheap and easily available, the catalytic performance is excellent, the catalytic life is long, the mechanical strength is high, and it has extremely high industrial application value and prospects.

[0048] In some embodiments, during the preparation of the modified iron-based metal oxide, the temperature (° C.) can be any value of 50, 55, 60, 65, 70, or a range consisting of any two values.

[0049] In some embodiments, during the preparation of the modified iron-based metal oxide, the aging time (h) can be any value of 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or a range consisting of any two values.

[0050] In some embodiments, during the preparation of the modified iron-based metal oxide, the calcination temperature (° C.) can be any value of 300, 350, 400, 450, 500, 550, or a range consisting of any two values.

[0051] In some embodiments, the calcination time (h) can be any value of 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, or a range consisting of any two values.

[0052] In some embodiments, during the preparation of HZSM-5 molecular sieve, the molar ratio of tetraethyl orthosilicate, tetrapropylammonium hydroxide, sodium aluminate and deionized water is 2: (0.01-1): (0.01-0.5): (40-60).

[0053] In some embodiments, the molecular weight of polyethylene glycol is any value selected from 2000, 4000, 6000, or a range consisting of any two values.

[0054] In some embodiments, based on the molar number of tetraethyl orthosilicate as 2, the molar ratio of tetraethyl orthosilicate to tetrapropylammonium hydroxide is any value of 2:0.01, 2:0.05, 2:0.1, 2:0.2, 2:0.3, 2:0.4, 2:0.5, 2:0.6, 2:0.7, 2:0.8, 2:0.9, 2:1.0, or a range consisting of any two values.

[0055] In some embodiments, based on the molar number of tetraethyl orthosilicate as 2, the molar ratio of tetraethyl orthosilicate to polyethylene glycol is any value of 2:0.001, 2:0.002, 2:0.003, 2:0.004, 2:0.005, 2:0.006, 2:0.007, 2:0.008, 2:0.009, 2:0.01, or a range consisting of any two values.

[0056] In some embodiments, the crystallization time (h) is any value of 12, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 72, or a range consisting of any two values.

[0057] In some embodiments, the crystallization temperature (° C.) is any value of 100, 110, 120, 130, 140, 150, 160, 170, 180, or a range consisting of any two values.

[0058] In some embodiments, during the preparation of HZSM-5 molecular sieve, the calcination time (h) is any value of 2, 3, 4, 5, 6, 7, 8, or a range consisting of any two values.

[0059] In some embodiments, during the preparation of HZSM-5 molecular sieve, the calcination temperature (° C.) is any value of 400, 450, 500, 550, 600 or a range consisting of any two values.

[0060] In some embodiments, the iron-based metal oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:(0.5-2) to obtain a composite catalyst.

[0061] In a third aspect, the embodiments of the present application further provide the use of the above-mentioned composite catalyst in the preparation of aromatics by hydrogenation of carbon dioxide.

[0062] In some embodiments, the above application is the application of the composite catalyst in the direct production of high value-added aromatics by hydrogenation of carbon dioxide.

[0063] In some embodiments, the high value-added aromatics include C6-C8 aromatics, mainly including benzene, toluene, and xylene (BTX).

[0064] In some embodiments, the above application includes the following steps: loading the composite catalyst into a reactor, introducing reducing gas hydrogen for reduction, and after the reduction is completed, introducing the reaction raw gas, the volume ratio of H2 to CO2 in the reaction raw gas is 3 to 9, the reaction temperature is 280 to 380°C, and the reaction pressure is 2.6 to 4MPa.

[0065] This application can be used for the development and production of downstream products of enterprises that generate a large amount of carbon dioxide during the production process. In addition, this application can achieve efficient coupling of multiple reactions in one reactor, breaking the limitation of the Fischer-Tropsch synthesis reaction by the ASF distribution law, making the reaction move in a direction that is conducive to the generation of the target product, minimizing the occurrence of side reactions, enhancing the positive driving force of the main reaction, reducing the selectivity of by-products, and maximizing the carbon dioxide conversion rate and the yield of product aromatics.

[0066] In some embodiments, the volume ratio of H2 to CO2 in the reaction raw material gas is any value of 3, 4, 5, 6, 7, 8, 9, or a range consisting of any two values.

[0067] In some embodiments, the reaction temperature (° C.) is any value of 280, 290, 300, 310, 320, 330, 340, 350, 360, 370, 380, or a range consisting of any two values.

[0068] In some embodiments, the reaction pressure (MPa) is any value of 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, or a range consisting of any two values.

[0069] In some embodiments, the space velocity of the reaction raw gas is 500 to 6000 h -1 The reaction time is 24 to 72 hours.

[0070] In some embodiments, the space velocity (h -1 ) is any value among 500, 1000, 2000, 3000, 4000, 5000, 6000, or a range consisting of any two values.

[0071] In some embodiments, the reaction time (h) is any value of 24, 30, 35, 40, 45, 50, 55, 60, 65, 70, 72, or a range consisting of any two values.

[0072] The reagents used in the examples of this application are shown in Table 1:

[0073] Table 1

[0074]

[0075]

[0076] Example 1

[0077] The first step, the preparation method of iron-zinc metal oxide comprises the following steps:

[0078] Add 150mL of deionized water to a beaker and place it in a 60°C constant temperature water bath. Pour 13.39g of iron nitrate nine hydrate and 29.53g of zinc nitrate hexahydrate solids into the beaker. Turn on the magnetic stirring to completely dissolve the solids to obtain a metal nitrate precursor solution. Prepare 1mol / L ammonia solution as a precipitant. Under a constant temperature of 60°C, slowly add ammonia solution to the precursor solution (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. Stop adding ammonia solution when the pH reaches 9.0-9.3. Keep the temperature constant and continue stirring to age the resulting suspension for 60 minutes.

[0079] The suspension was washed and filtered until the filtrate was neutral, the filter cake was dried at 110°C, and calcined at 400°C for 4 hours to obtain an iron-zinc bimetallic oxide, wherein the molar ratio of iron to zinc was 1:3. The obtained iron-zinc bimetallic oxide was ball-milled to less than 1000 mesh for subsequent impregnation.

[0080] Weigh 4 g of sodium carbonate and prepare a sodium carbonate solution with 4 mL of deionized water. Impregnate the iron-zinc bimetallic oxide in the sodium carbonate solution. After impregnation, let it stand for 24 hours and dry it at 110° C. for 12 hours to obtain a sodium-modified iron-zinc bimetallic oxide.

[0081] The sodium-modified iron-zinc bimetallic oxide is an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified bimetallic oxide is 0.2326 cm 3 / g, specific surface area is 18.2561m 2 / g, average pore size is 14.3567nm;

[0082] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method:

[0083] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, 0.5g of polyethylene glycol, and 45g of deionized water to make a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, hydrothermally crystallize for 48h, and the hydrothermal crystallization temperature is 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0084] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0085] The pore volume of HZSM-5 molecular sieve is 0.326 cm 3 / g, specific surface area is 322m 2 / g, the average pore size is 6.15nm, and the silicon-aluminum ratio is 25.

[0086] The third step is to prepare a sodium-modified iron-zinc bimetallic oxide and HZSM-5 molecular sieve composite catalyst by physical mixing:

[0087] The sodium-modified iron-zinc bimetallic oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:1. After being fully mixed, a composite catalyst for directly producing high-value-added aromatics by hydrogenating carbon dioxide is obtained.

[0088] Determination of catalyst structure:

[0089] (1) The size and morphology of the prepared metal oxides were determined by scanning electron microscopy and transmission electron microscopy.

[0090] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0091] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics by hydrogenation of carbon dioxide:

[0092] The performance evaluation of the composite catalyst was carried out in a fixed-bed tubular reactor. 2g of the composite catalyst was placed in the constant temperature section of the reaction tube, and then the temperature was raised from room temperature to the reduction temperature at 2°C / min in a nitrogen environment. The reducing gas flow rate was 100mL / min, and the reduction conditions were: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction was completed, the temperature in the fixed-bed tubular reactor was adjusted to the reaction temperature, and the reaction raw gas was switched. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas was 3, the temperature was 320°C, the pressure was 3MPa, and the space velocity was 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0093] Example 2

[0094] The first step, the preparation method of iron-zinc metal oxide comprises the following steps:

[0095] Add 150mL of deionized water to a beaker and place it in a 60°C constant temperature water bath. Pour 24.10g of iron nitrate nine hydrate and 17.72g of zinc nitrate hexahydrate solids into the beaker. Turn on the magnetic stirring to completely dissolve the solids to obtain a metal nitrate precursor solution. Prepare 1mol / L ammonia solution as a precipitant. Under a constant temperature of 60°C, slowly add ammonia solution to the precursor solution (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. Stop adding ammonia solution when the pH reaches 9.0-9.3. Keep the temperature constant and continue stirring to age the resulting suspension for 60 minutes.

[0096] The suspension was washed and filtered until the filtrate was neutral, the filter cake was dried at 110°C, and calcined at 400°C for 4 hours to obtain an iron-zinc bimetallic oxide, wherein the molar ratio of iron to zinc was 1:1. The obtained iron-zinc bimetallic oxide was ball-milled to less than 1000 mesh for subsequent impregnation.

[0097] Weigh 4 g of sodium carbonate and prepare a sodium carbonate solution with 4 mL of deionized water. Impregnate the iron-zinc bimetallic oxide in the sodium carbonate solution. After impregnation, let it stand for 24 hours and dry it at 110° C. for 12 hours to obtain a sodium-modified iron-zinc bimetallic oxide.

[0098] The sodium-modified iron-zinc bimetallic oxide is an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified bimetallic oxide is 0.2538 cm 3 / g, specific surface area is 23.2631m 2 / g, average pore size is 31.2321nm;

[0099] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method:

[0100] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, 0.5g of polyethylene glycol, and 45g of deionized water to make a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, hydrothermally crystallize for 48h, and the hydrothermal crystallization temperature is 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0101] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0102] The pore volume of HZSM-5 molecular sieve is 0.326 cm 3 / g, specific surface area is 322m 2 / g, the average pore size is 6.15nm, and the silicon-aluminum ratio is 25.

[0103] The third step is to prepare a sodium-modified iron-zinc bimetallic oxide and HZSM-5 molecular sieve composite catalyst by physical mixing:

[0104] The sodium-modified iron-zinc bimetallic oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:1. After being fully mixed, a composite catalyst for directly producing high-value-added aromatics by hydrogenating carbon dioxide is obtained.

[0105] Determination of catalyst structure:

[0106] (1) Determine the size and morphology of the prepared metal oxide by scanning electron microscopy and transmission electron microscopy;

[0107] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0108] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics by hydrogenation of carbon dioxide:

[0109] The performance evaluation of the composite catalyst was carried out in a fixed-bed tubular reactor. 2g of the composite catalyst was placed in the constant temperature section of the reaction tube, and then the temperature was raised from room temperature to the reduction temperature at 2°C / min in a nitrogen environment. The reducing gas flow rate was 100mL / min, and the reduction conditions were: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction was completed, the temperature in the fixed-bed tubular reactor was adjusted to the reaction temperature, and the reaction raw gas was switched. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas was 3, the temperature was 320°C, the pressure was 3MPa, and the space velocity was 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0110] Example 3

[0111] The first step, the preparation method of iron-zinc metal oxide comprises the following steps:

[0112] Add 150mL of deionized water to a beaker and place it in a 60°C constant temperature water bath. Pour 24.10g of iron nitrate nine hydrate and 5.90g of zinc nitrate hexahydrate solids into the beaker. Turn on the magnetic stirring to completely dissolve the solids to obtain a metal nitrate precursor solution. Prepare 1mol / L ammonia solution as a precipitant. Under a constant temperature of 60°C, slowly add ammonia solution to the precursor solution (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. When the pH reaches 9.0-9.3, stop adding ammonia solution, keep the temperature unchanged and continue stirring, and age the resulting suspension for 60 minutes.

[0113] The suspension was washed and filtered until the filtrate was neutral, the filter cake was dried at 110°C, and calcined at 400°C for 4 hours to obtain an iron-zinc bimetallic oxide, wherein the molar ratio of iron to zinc was 3:1. The obtained iron-zinc bimetallic oxide was ball-milled to less than 1000 mesh for subsequent impregnation.

[0114] Weigh 4 g of sodium carbonate and prepare a sodium carbonate solution with 4 mL of deionized water. Impregnate the iron-zinc bimetallic oxide in the sodium carbonate solution. After impregnation, let it stand for 24 hours and dry it at 110° C. for 12 hours to obtain a sodium-modified iron-zinc bimetallic oxide.

[0115] The sodium-modified iron-zinc bimetallic oxide is an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified bimetallic oxide is 0.2021 cm 3 / g, specific surface area is 39.8431m 2 / g, average pore size is 17.6385nm;

[0116] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method:

[0117] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, 0.5g of polyethylene glycol, and 45g of deionized water to make a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, hydrothermally crystallize for 48h, and the hydrothermal crystallization temperature is 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0118] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0119] The pore volume of HZSM-5 molecular sieve is 0.326 cm 3 / g, specific surface area is 322m 2 / g, the average pore size is 6.15nm, and the silicon-aluminum ratio is 25.

[0120] The third step is to prepare a sodium-modified iron-zinc bimetallic oxide and HZSM-5 molecular sieve composite catalyst by physical mixing:

[0121] The sodium-modified iron-zinc bimetallic oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:1. After being fully mixed, a composite catalyst for directly producing high-value-added aromatics by hydrogenating carbon dioxide is obtained.

[0122] Determination of catalyst structure:

[0123] (1) Determine the size and morphology of the prepared metal oxide by scanning electron microscopy and transmission electron microscopy;

[0124] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0125] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics by hydrogenation of carbon dioxide:

[0126] The performance evaluation of the composite catalyst was carried out in a fixed-bed tubular reactor. 2g of the composite catalyst was placed in the constant temperature section of the reaction tube, and then the temperature was raised from room temperature to the reduction temperature at 2°C / min in a nitrogen environment. The reducing gas flow rate was 100ml / min. The reduction conditions were: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction was completed, the temperature in the fixed-bed tubular reactor was adjusted to the reaction temperature, and the reaction raw gas was switched. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas was 3, the temperature was 320°C, the pressure was 3MPa, and the space velocity was 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0127] Example 4

[0128] The first step, the preparation method of iron-zinc metal oxide comprises the following steps:

[0129] Add 150mL of deionized water to a beaker and place it in a 60℃ constant temperature water bath. Pour 24.10g of iron nitrate nine hydrate and 3.54g of zinc nitrate hexahydrate solids into the beaker. Turn on the magnetic stirring to completely dissolve the solids to obtain a metal nitrate precursor solution. Prepare 1mol / L ammonia solution as a precipitant. At a constant temperature of 60℃, slowly add ammonia solution to the precursor solution (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. Stop adding ammonia solution when the pH reaches 9.0-9.3. Keep the temperature constant and continue stirring to age the resulting suspension for 60 minutes.

[0130] The suspension was washed and filtered until the filtrate was neutral, the filter cake was dried at 110°C, and calcined at 400°C for 4 hours to obtain an iron-zinc bimetallic oxide, wherein the molar ratio of iron to zinc was 5:1. The obtained iron-zinc bimetallic oxide was ball-milled to less than 1000 mesh for subsequent impregnation.

[0131] Weigh 4 g of sodium carbonate and prepare a sodium carbonate solution with 4 mL of deionized water. Impregnate the iron-zinc bimetallic oxide in the sodium carbonate solution. After impregnation, let it stand for 24 hours and dry it at 110° C. for 12 hours to obtain a sodium-modified iron-zinc bimetallic oxide.

[0132] The sodium-modified iron-zinc bimetallic oxide is an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified bimetallic oxide is 0.2836 cm 3 / g, specific surface area is 31.2328m 2 / g, the average pore size is 26.2354nm;

[0133] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method:

[0134] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, 0.5g of polyethylene glycol, and 45g of deionized water to make a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, hydrothermally crystallize for 48h, and the hydrothermal crystallization temperature is 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0135] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0136] The pore volume of HZSM-5 molecular sieve is 0.326 cm 3 / g, specific surface area is 322m 2 / g, the average pore size is 6.15nm, and the silicon-aluminum ratio is 25.

[0137] The third step is to prepare a sodium-modified iron-zinc bimetallic oxide and HZSM-5 molecular sieve composite catalyst by physical mixing:

[0138] The sodium-modified iron-zinc bimetallic oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:1. After being fully mixed, a composite catalyst for directly producing high-value-added aromatics by hydrogenating carbon dioxide is obtained.

[0139] Determination of catalyst structure:

[0140] (1) Determine the size and morphology of the prepared metal oxide by scanning electron microscopy and transmission electron microscopy;

[0141] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0142] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics by hydrogenation of carbon dioxide:

[0143] The performance evaluation of the composite catalyst was carried out in a fixed-bed tubular reactor. 2g of the composite catalyst was placed in the constant temperature section of the reaction tube, and then the temperature was raised from room temperature to the reduction temperature at 2°C / min in a nitrogen environment. The reducing gas flow rate was 100mL / min, and the reduction conditions were: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction was completed, the temperature in the fixed-bed tubular reactor was adjusted to the reaction temperature, and the reaction raw gas was switched. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas was 3, the temperature was 320°C, the pressure was 3MPa, and the space velocity was 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0144] Example 5

[0145] The first step, the preparation method of iron-zinc metal oxide comprises the following steps:

[0146] Add 150mL of deionized water to a beaker and place it in a 60°C constant temperature water bath. Pour 24.10g of iron nitrate nine hydrate and 2.21g of zinc nitrate hexahydrate solids into the beaker. Turn on the magnetic stirring to completely dissolve the solids to obtain a metal nitrate precursor solution. Prepare 1mol / L ammonia solution as a precipitant. At a constant temperature of 60°C, slowly add ammonia solution to the precursor solution (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. When the pH reaches 9.0-9.3, stop adding ammonia solution, keep the temperature unchanged and continue stirring, and age the resulting suspension for 60 minutes.

[0147] The suspension was washed and filtered until the filtrate was neutral, the filter cake was dried at 110°C, and calcined at 400°C for 4 hours to obtain an iron-zinc bimetallic oxide, wherein the molar ratio of iron to zinc was 8:1. The obtained iron-zinc bimetallic oxide was ball-milled to less than 1000 mesh for subsequent impregnation.

[0148] Weigh 4 g of sodium carbonate and prepare a sodium carbonate solution with 4 mL of deionized water. Impregnate the iron-zinc bimetallic oxide in the sodium carbonate solution. After impregnation, let it stand for 24 hours and dry it at 110° C. for 12 hours to obtain a sodium-modified iron-zinc bimetallic oxide.

[0149] The sodium-modified iron-zinc bimetallic oxide is an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified bimetallic oxide is 0.2964 cm 3 / g, specific surface area is 33.2834m 2 / g, average pore size is 41.5163nm;

[0150] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method:

[0151] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, 0.5g of polyethylene glycol, and 45g of deionized water to make a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, hydrothermally crystallize for 48h, and the hydrothermal crystallization temperature is 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0152] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0153] The pore volume of HZSM-5 molecular sieve is 0.326 cm 3 / g, specific surface area is 322m 2 / g, the average pore size is 6.15nm, and the silicon-aluminum ratio is 25.

[0154] The third step is to prepare a sodium-modified iron-zinc bimetallic oxide and HZSM-5 molecular sieve composite catalyst by physical mixing:

[0155] The sodium-modified iron-zinc bimetallic oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:1. After being fully mixed, a composite catalyst for directly producing high-value-added aromatics by hydrogenating carbon dioxide is obtained.

[0156] Determination of catalyst structure:

[0157] (1) Determine the size and morphology of the prepared metal oxide by scanning electron microscopy and transmission electron microscopy;

[0158] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0159] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics by hydrogenation of carbon dioxide:

[0160] The performance evaluation of the composite catalyst was carried out in a fixed-bed tubular reactor. 2g of the composite catalyst was placed in the constant temperature section of the reaction tube, and then the temperature was raised from room temperature to the reduction temperature at 2°C / min in a nitrogen environment. The reducing gas flow rate was 100mL / min, and the reduction conditions were: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction was completed, the temperature in the fixed-bed tubular reactor was adjusted to the reaction temperature, and the reaction raw gas was switched. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas was 3, the temperature was 320°C, the pressure was 3MPa, and the space velocity was 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0161] Comparative Example 1

[0162] The first step is to prepare the iron-based metal oxide by the method comprising the following steps (without transition metal modification):

[0163] Add 24.10g of solid ferric nitrate nine hydrate to 150mL of deionized water, place in a constant temperature water bath, stir and heat continuously to completely dissolve it to obtain a precursor solution. Weigh ammonia solution and dilute with water to prepare a precipitant with a concentration of 1mol / L. Slowly add ammonia solution to the precursor solution at a constant temperature of 60°C (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. Stop adding ammonia solution when the pH reaches 9.0-9.3, keep the temperature unchanged and continue stirring, and age the resulting suspension for 60 minutes.

[0164] The suspension was filtered and washed with quantitative deionized water until the filtrate obtained by filtration was neutral, the filter cake obtained by filtration was dried at 110°C, and the dried solid was calcined at 400°C for 4h to obtain pure iron-based metal oxide. The obtained iron-based metal oxide was ball-milled to less than 1000 mesh for subsequent impregnation process.

[0165] Weigh 4 g of sodium carbonate and prepare a sodium carbonate solution with 4 mL of deionized water. Impregnate the above pure iron-based metal oxide in the sodium carbonate solution. After impregnation, let it stand for 24 hours and dry it at 110° C. for 12 hours to obtain a sodium-modified iron-based metal oxide.

[0166] The sodium-modified iron-based metal oxide is in the form of an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified metal oxide is 0.1839 cm 3 / g, specific surface area is 21.9639m 2 / g, average pore size is 33.4963nm;

[0167] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method:

[0168] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, 0.5g of polyethylene glycol, and 45g of deionized water to make a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, hydrothermally crystallize for 48h, and the hydrothermal crystallization temperature is 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0169] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0170] The pore volume of HZSM-5 molecular sieve is 0.326 cm 3 / g, specific surface area is 322m 2 / g, the average pore size is 6.15nm, and the silicon-aluminum ratio is between 20 and 150.

[0171] The third step is to prepare a sodium-modified iron-based metal oxide and HZSM-5 molecular sieve composite catalyst by physical mixing:

[0172] The sodium-modified iron-based metal oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:1. After being fully mixed, a composite catalyst for directly producing high-value-added aromatics by hydrogenating carbon dioxide is obtained.

[0173] Determination of catalyst structure:

[0174] (1) Determine the size and morphology of the prepared metal oxide by scanning electron microscopy and transmission electron microscopy;

[0175] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0176] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics from carbon dioxide:

[0177] Weigh 2g of the composite catalyst for directly producing high value-added aromatics from carbon dioxide and load it into the constant temperature section of the fixed-bed tubular reactor. Then, in a nitrogen environment, heat the room temperature to the reduction temperature at 2°C / min. The reducing gas flow rate is 100ml / min. The reduction conditions are: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction is completed, adjust the temperature in the fixed-bed tubular reactor to the reaction temperature and switch the reaction raw gas. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas is 3, the temperature is 320°C, the pressure is 3MPa, and the space velocity is 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0178] Comparative Example 2

[0179] The first step, the preparation method of iron-zinc metal oxide comprises the following steps (without alkali metal modification):

[0180] Add 150mL of deionized water to a beaker and place it in a 60°C constant temperature water bath. Pour 24.10g of iron nitrate nine hydrate and 5.90g of zinc nitrate hexahydrate solids into the beaker. Turn on the magnetic stirring to completely dissolve the solids to obtain a metal nitrate precursor solution. Prepare 1mol / L ammonia solution as a precipitant. Under a constant temperature of 60°C, slowly add ammonia solution to the precursor solution (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. When the pH reaches 9.0-9.3, stop adding ammonia solution, keep the temperature unchanged and continue stirring, and age the resulting suspension for 60 minutes.

[0181] The suspension was washed and filtered until the filtrate was neutral, the filter cake was dried at 110°C, and calcined at 400°C for 4 hours to obtain an iron-zinc bimetallic oxide, in which the molar ratio of iron to zinc elements was 3:1.

[0182] The alkali-free iron-zinc bimetallic oxide is an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified metal oxide is 0.1754 cm 3 / g, specific surface area is 44.5701m 2 / g, average pore size is 15.7413nm;

[0183] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method:

[0184] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, 0.5g of polyethylene glycol, and 45g of deionized water to make a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, hydrothermally crystallize for 48h, and the hydrothermal crystallization temperature is 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0185] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0186] The pore volume of HZSM-5 molecular sieve is 0.326 cm 3 / g, specific surface area is 322m 2 / g, the average pore size is 6.15nm, and the silicon-aluminum ratio is between 20 and 150.

[0187] The third step is to prepare a composite catalyst of iron-zinc metal oxide and HZSM-5 molecular sieve modified without alkali metal additive by physical mixing:

[0188] The iron-zinc metal oxide modified without alkali metal additive and the HZSM-5 molecular sieve are sieved to 40-60 mesh respectively, and the two are physically mixed at a mass ratio of 1:1. After fully mixing, a composite catalyst for directly producing high-value-added aromatics by hydrogenating carbon dioxide is obtained.

[0189] Determination of catalyst structure:

[0190] (1) Determine the size and morphology of the prepared metal oxide by scanning electron microscopy and transmission electron microscopy;

[0191] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0192] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics by hydrogenation of carbon dioxide:

[0193] The performance evaluation of the composite catalyst was carried out in a fixed-bed tubular reactor. 2g of the composite catalyst was placed in the constant temperature section of the reaction tube, and then the temperature was raised from room temperature to the reduction temperature at 2°C / min in a nitrogen environment. The reducing gas flow rate was 100mL / min, and the reduction conditions were: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction was completed, the temperature in the fixed-bed tubular reactor was adjusted to the reaction temperature, and the reaction raw gas was switched. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas was 3, the temperature was 320°C, the pressure was 3MPa, and the space velocity was 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0194] Comparative Example 3

[0195] The first step, the preparation method of iron-zinc metal oxide comprises the following steps:

[0196] Add 150mL of deionized water to a beaker and place it in a 60°C constant temperature water bath. Pour 24.10g of iron nitrate nine hydrate and 5.90g of zinc nitrate hexahydrate solids into the beaker. Turn on the magnetic stirring to completely dissolve the solids to obtain a metal nitrate precursor solution. Prepare 1mol / L ammonia solution as a precipitant. Under a constant temperature of 60°C, slowly add ammonia solution to the precursor solution (at a rate of one drop per three seconds), and keep stirring. Monitor the pH of the solution with a pH meter. When the pH reaches 9.0-9.3, stop adding ammonia solution, keep the temperature unchanged and continue stirring, and age the resulting suspension for 60 minutes.

[0197] The suspension was washed and filtered until the filtrate was neutral, the filter cake was dried at 110°C, and calcined at 400°C for 4 hours to obtain an iron-zinc bimetallic oxide, wherein the molar ratio of iron to zinc was 3:1. The obtained iron-zinc bimetallic oxide was ball-milled to less than 1000 mesh for subsequent impregnation.

[0198] Weigh 4 g of sodium carbonate and prepare a sodium carbonate solution with 4 mL of deionized water. Impregnate the iron-zinc bimetallic oxide in the sodium carbonate solution. After impregnation, let it stand for 24 hours and dry it at 110° C. for 12 hours to obtain a sodium-modified iron-zinc bimetallic oxide.

[0199] The sodium-modified iron-zinc bimetallic oxide is an amorphous powder with a particle size of less than 12 μm. The pore volume of the sodium-modified bimetallic oxide is 0.2021 cm 3 / g, specific surface area is 39.8431m 2 / g, average pore size is 17.6385nm;

[0200] The second step is to prepare HZSM-5 molecular sieve by dynamic hydrothermal method (without introducing structural additive PEG2000):

[0201] Weigh 20.833g of tetraethyl orthosilicate, 15.252g of tetrapropylammonium hydroxide, and 45g of deionized water to mix and prepare a molecular sieve precursor solution. Stir at room temperature for 24h. After sufficient hydrolysis and dispersion, determine the mass of sodium aluminate to be 0.328g according to the molar ratio of tetraethyl orthosilicate to sodium aluminate of 2:0.08, and add it to the above-mentioned silicon precursor solution after sufficient hydrolysis and dispersion, stir at room temperature for 5h, fully disperse, transfer the suspension to a hydrothermal crystallization kettle, and hydrothermally crystallize for 48h at a hydrothermal crystallization temperature of 170°C. During this period, the crystallization kettle rotates at a rate of 45r / min. The crystallized product is centrifugally washed and dried at 110°C for 12h. The solid powder obtained after drying is calcined at 550°C for 5h to obtain a Na-type ZSM-5 molecular sieve.

[0202] Prepare 1 mol / L ammonium chloride solution, grind Na-type ZSM-5 molecular sieve into powder and pour into the above solution, stir at 80°C for 3 hours and then filter, dry the filter cake at 110°C for 12 hours, repeat the above process twice, grind the final solid into powder and calcine at 550°C for 5 hours to obtain HZSM-5 molecular sieve;

[0203] The pore volume of HZSM-5 molecular sieve is 0.283 cm 3 / g, specific surface area is 310m 2 / g, the average pore size is 5.85nm, and the silicon-aluminum ratio is 25.

[0204] The third step is to prepare a sodium-modified iron-zinc bimetallic oxide and HZSM-5 molecular sieve composite catalyst by physical mixing:

[0205] The sodium-modified iron-zinc bimetallic oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:1. After being fully mixed, a composite catalyst for directly producing high-value-added aromatics from carbon dioxide is obtained.

[0206] Determination of catalyst structure:

[0207] (1) Determine the size and morphology of the prepared metal oxide by scanning electron microscopy and transmission electron microscopy;

[0208] (2) The morphology and structure of HZSM-5 molecular sieve prepared by dynamic hydrothermal method were determined by scanning electron microscopy and transmission electron microscopy.

[0209] Step 4: Evaluation of the catalytic performance of the composite catalyst for direct production of high value-added aromatics by hydrogenation of carbon dioxide:

[0210] The performance evaluation of the composite catalyst was carried out in a fixed-bed tubular reactor. 2g of the composite catalyst was placed in the constant temperature section of the reaction tube, and then the temperature was raised from room temperature to the reduction temperature at 2°C / min in a nitrogen environment. The reducing gas flow rate was 100mL / min, and the reduction conditions were: pure hydrogen at normal pressure and a temperature of 350°C for 10h. After the reduction was completed, the temperature in the fixed-bed tubular reactor was adjusted to the reaction temperature, and the reaction raw gas was switched. Reaction conditions: The volume ratio of H2 to CO2 in the reaction raw gas was 3, the temperature was 320°C, the pressure was 3MPa, and the space velocity was 1200h. -1 The reaction time was 48 h. The reaction results are shown in Table 2.

[0211] Table 2

[0212]

[0213] In Table 2, CO2 conv. represents the CO2 conversion rate, CO sel. represents the selectivity of CO in all products, Hydrocarbon sel. represents the selectivity of various hydrocarbons in total hydrocarbons, CH4, C2-C4, Aliphatics, Aro. represent the selectivity of methane, C2-C4 hydrocarbons, aliphatics, and aromatics in total hydrocarbons, respectively, and C 5+ sel. indicates various C 5+ Hydrocarbons in C 5+ Selectivity in total hydrocarbons, Aliphatics means C 5+ The selectivity of aliphatic hydrocarbons in total hydrocarbons, Aro.L represents C 5+ Selectivity of aromatics in total hydrocarbons.

[0214] As shown in Table 2, the modified bimetallic oxide catalyst prepared by the present invention is coupled with HZSM-5 molecular sieve by physical mixing to realize the direct production of aromatics from carbon dioxide. By changing the iron-zinc ratio in the iron-zinc bimetallic oxide and adding metal additives, the product distribution can be adjusted to increase C 5+ The selectivity of total hydrocarbons increases the selectivity of aromatics in C 5+ The selectivity in total hydrocarbons significantly increases the carbon dioxide conversion rate. Figure 1 The composite catalyst prepared by physically mixing iron-zinc bimetallic oxide with different iron-zinc metal ratios and HZSM-5 molecular sieve is used for the catalytic performance of direct production of high value-added aromatics from carbon dioxide. In addition, the introduction of structural additive polyethylene glycol into the HZSM-5 molecular sieve can further improve the selectivity of aromatic products in total hydrocarbons. Compared with the iron-based oxide catalyst in Comparative Example 1, the iron-zinc bimetallic oxide catalyst prepared in this application has a higher carbon dioxide conversion rate and a lower gaseous hydrocarbon selectivity. 5+On the other hand, compared with Comparative Example 2, the introduction of the metal additive sodium into the iron-zinc bimetallic oxide can greatly improve the carbon dioxide conversion rate. In addition, the selectivity of aromatic hydrocarbons in the total hydrocarbons is also greatly improved. Compared with the HZSM-5 molecular sieve preparation process in Comparative Example 3 without the addition of polyethylene glycol structural additive, the HZSM-5 molecular sieve after adding polyethylene glycol structural additive can further improve C 5+ The selectivity of aromatics in total hydrocarbons is also improved, and the selectivity of aromatics in total hydrocarbons is also improved, and the catalyst's aromatic selectivity (the catalyst can generate a variety of products by catalyzing carbon dioxide, and the structural shape and molecular size of each product are different. Therefore, the closer the pore structure of the catalyst is to a certain product, the greater the selectivity of this product in the product, that is, the selectivity). During the reaction, the carbon dioxide conversion rate can reach 42%, the by-product CO selectivity can be controlled within 7%, and the total aromatic selectivity can reach 63%. In the liquid phase C 5+ The selectivity in hydrocarbon products exceeds 80%. The composite catalyst obtained by physically mixing the metal promoter-modified iron-zinc bimetallic oxide catalyst prepared in the present application and the HZSM-5 molecular sieve synthesized by dynamic hydrothermal method has better catalytic performance than the traditional iron-based catalyst.

[0215] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0216] The above is a detailed introduction to a composite catalyst provided in the embodiments of the present application, its preparation method and application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A composite catalyst, characterized in that: The composite catalyst comprises a modified iron-based metal oxide and a HZSM-5 molecular sieve; The molar ratio of iron to zinc in the modified iron-based metal oxide is 1:(1-8); the modified iron-based metal oxide includes a metal additive, and the metal additive includes at least one element selected from the group consisting of sodium, potassium, zinc, manganese, and copper; the mass percentage of the metal additive in the composite catalyst is 0.5%-8%; The HZSM-5 molecular sieve includes a structural additive, and the mass percentage of the structural additive to the HZSM-5 molecular sieve is 1-2%; the structural additive includes polyethylene glycol; The mass ratio of the modified iron-based metal oxide to the HZSM-5 molecular sieve is 1:(0.5-2); The preparation method of the composite catalyst comprises the following steps: Preparation of modified iron-based metal oxide: at a temperature of 50-70° C., an alkaline precipitant is added dropwise to a solution of iron nitrate and zinc nitrate in a molar ratio of 1:(1-8); when the pH reaches 3.2-12, the titration endpoint is reached, and the solution is aged for 0.5-5 hours. After the aging is completed, the obtained reaction product is filtered, washed, and dried; the dried reaction product is calcined at 300-550° C. for 4-8 hours to obtain an iron-based metal oxide, the iron-based metal oxide is loaded with a metal additive by an impregnation method, the obtained product is dried, and calcined at 300-550° C. for 4-8 hours to obtain a modified iron-based metal oxide; Preparation of HZSM-5 molecular sieve: tetraethyl orthosilicate, tetrapropylammonium hydroxide and polyethylene glycol in a molar ratio of 2: (0.01-2): (0-0.01) are mixed with deionized water to prepare a molecular sieve silicon source precursor solution, sodium aluminate is added to the molecular sieve silicon source precursor solution to obtain a suspension, the suspension is subjected to hydrothermal crystallization for 12-72 hours, the crystallization temperature is controlled at 100-180° C., the product obtained after the crystallization is completed is centrifuged and washed until the pH is neutral, dried and calcined, the calcination time is 2-8 hours, and the calcination temperature is 400-600° C. to obtain a Na-type ZSM-5 molecular sieve; the Na-type ZSM-5 molecular sieve is poured into an NH4Cl solution and stirred, the temperature is controlled at 50-100° C., ion exchange is performed for 2-4 hours, and then centrifuged and washed and dried, and calcined at 400-600° C. for 2-8 hours to obtain a HZSM-5 molecular sieve; The modified iron-based metal oxide and the HZSM-5 molecular sieve are mixed to obtain a composite catalyst.

2. The composite catalyst according to claim 1, characterized in that The pore volume of the HZSM-5 molecular sieve is 0.1~60cm 3 / g, specific surface area is 150~500m 2 / g, the average pore size is 5~100nm, and the silicon-aluminum ratio is 20~150.

3. The composite catalyst according to claim 1, characterized in that The pore volume of the modified iron-based metal oxide is 0.10-0.45 cm 3 / g, with a specific surface area of ​​15~50m 2 / g, pore size is 10~60nm.

4. The composite catalyst according to claim 1, characterized in that The modified iron-based metal oxide and the HZSM-5 molecular sieve are sieved to 40-60 meshes respectively, and the two are physically mixed at a mass ratio of 1:(0.5-2) to obtain a composite catalyst.

5. Use of the composite catalyst as claimed in any one of claims 1 to 4 in the preparation of aromatic hydrocarbons by hydrogenation of carbon dioxide.

6. The use according to claim 5, characterized in that: The method comprises the following steps: loading the composite catalyst into a reactor, introducing reducing gas hydrogen for reduction, and after the reduction is completed, introducing a reaction raw gas, wherein the volume ratio of H2 to CO2 in the reaction raw gas is 3-9, the reaction temperature is 280-380°C, and the reaction pressure is 2.6-4MPa.

7. The use according to claim 6, characterized in that: The space velocity of the reaction raw gas is 500~6000h -1 The reaction time is 24~72h.