A PBT composite material and its preparation method and application

By adding specific components such as diethyl aluminum hypophosphate, phosphazene-free halogen-free flame retardant synergistic agent to the PBT composite material, the problem of low laser transmittance of PBT resin is solved, and thin-wall flame retardant and laser welding are achieved The overall performance of the material is improved.

CN116515258BActive Publication Date: 2024-11-19KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310454918.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-19
Estimated Expiration
2043-04-25

AI Technical Summary

Technical Problem

Due to its low laser transmittance, PBT resin is difficult to be used directly for laser welding. In the prior art, the addition of amorphous resin to improve laser transmittance will affect the heat resistance of the material, limiting its application range, especially for For halogen-free flame retardant systems, laser welding technology is more difficult.

Method used

By adding diethyl aluminum hypophosphate, phosphazene halogen-free flame retardant synergist, polyethylene glycol and epoxy chain extenders to the PBT composite material, combined with specific group distribution ratios and preparation processes, thin-wall flame retardant is formed. and laser-weldable PBT composites.

Benefits of technology

The thin-wall flame retardancy of PBT composite materials is achieved and the advantages of being suitable for laser welding, while maintaining the heat resistance and application range of the material, and having excellent laser transmittance and melt flowability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a PBT composite material, which comprises the following components by weight: 50 parts of PBT resin; 8-16 parts of diethyl aluminum phosphite; 3-7 parts of phosphazene halogen-free flame retardant synergist; 1-4 parts of polyethylene glycol; 0.1-0.3 parts of epoxy chain extender; the average molecular weight of the polyethylene glycol is 1000-4000. On the one hand, the present invention selects a composite flame retardant of diethyl aluminum phosphite / phosphazene halogen-free flame retardant synergist, which not only has good flame retardancy, but also has less absorption of 980nm laser. On the other hand, by selecting polyethylene glycol and epoxy chain extender with a specific average molecular weight, the crystallization ability of PBT can be enhanced, the thickness of the wafer can be reduced, thereby effectively reducing laser absorption, and the fluidity can be improved to achieve thin-wall flame retardancy. The PBT composite material of the present invention has the advantages of good thin-wall flame retardancy and being suitable for laser welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a PBT composite material and a preparation method and application thereof. Background Art

[0002] Polybutylene terephthalate (PBT) is a crystalline saturated polyester with the advantages of high temperature resistance, moisture resistance, good electrical insulation, oil resistance, chemical corrosion resistance, and fast molding. PBT is widely used in the fields of electronics, automobiles, machinery, lighting, etc. In recent years, halogen-free flame-retardant PBT has the advantages of environmental protection and low pollution, and is the current research technical difficulty and hot spot. In the fields of electronics and automobiles, laser welding technology has received more and more attention. Compared with other traditional welding technologies, laser welding has the advantages of fast speed, large depth, small deformation, etc., and can be welded at room temperature or under special conditions. However, PBT resin is a semi-crystalline resin with low laser transmittance, so it is difficult to use it directly for laser welding.

[0003] In the existing invention technology, there are generally two ways to improve the laser welding ability of PBT. One is to add non-crystalline resin. For example, patents CN104910620, CN108473668, CN109401219 and CN109233216 all add non-crystalline resin to semi-crystalline resin, thereby weakening the crystallization ability of crystalline resin to improve laser transmittance; however, adding non-crystalline resin will directly affect the heat resistance of the material and limit the application range of the material. The above research on laser transmittance of PBT has rarely been studied for PBT halogen-free flame retardant system, and the technical difficulty of ultra-thin halogen-free flame retardant and laser weldable is relatively large. Summary of the invention

[0004] The object of the present invention is to provide a PBT composite material with thin-wall flame retardancy and laser weldability.

[0005] The present invention is achieved through the following technical solutions:

[0006] A PBT composite material, comprising the following components in parts by weight:

[0007] 50 parts of PBT resin;

[0008] 8-16 parts of diethyl aluminum hypophosphite;

[0009] 3-7 parts of phosphazene halogen-free flame retardant synergist;

[0010] 1-4 parts of polyethylene glycol;

[0011] Epoxy chain extender 0.1-0.3 parts;

[0012] The average molecular weight of the polyethylene glycol is 1000-4000.

[0013] Preferably, the following components are included in parts by weight:

[0014] 50 parts of PBT resin;

[0015] 8-16 parts of diethyl aluminum hypophosphite;

[0016] 3-7 parts of phosphazene halogen-free flame retardant synergist;

[0017] 1.5-3.5 parts of polyethylene glycol;

[0018] Epoxy chain extender 0.15-0.25 parts.

[0019] The phosphazene halogen-free flame retardant synergist is selected from at least one of hexaphenoxy cyclotriphosphazene, monocyanophenoxy pentaphenoxy cyclotriphosphazene, dicyanophenoxy tetraphenoxy cyclotriphosphazene and tricyanophenoxy triphenoxy cyclotriphosphazene.

[0020] The epoxy chain extender is selected from at least one of bisphenol A diglycidyl ether and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate.

[0021] Preferably, the mass content of the epoxy chain extender in the PBT composite material is 0.1 wt %-0.45 wt %, more preferably 0.15 wt %-0.41 wt %.

[0022] Preferably, the average molecular weight of the polyethylene glycol is 2000-3000.

[0023] The intrinsic viscosity of the PBT resin is in the range of 0.6-1.2 dL / g (test condition is 25° C., test standard GB / T1632.1-2008).

[0024] Preferably, in order to further improve the flame retardancy of the thin wall, 0-1.5 parts of pentaerythritol phosphate are also included by weight. Pentaerythritol phosphate can also be used as a carbon source, dehydrated into carbon by esterification reaction, reduce oxygen concentration, take away heat, release inert gas to expand, form a uniform carbon layer, and insulate heat, isolate oxygen, suppress smoke, and resist dripping.

[0025] It is possible to choose whether to add 0-1 part of antioxidant according to actual needs. It can be a hindered phenol antioxidant, specifically one of β (3,5 di-tert-butyl-4-hydroxyphenyl) propionate or 1,3,5-tris (4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl) -1,3,5-triazine-2,4,6-(1H,3H,5H)-trione.

[0026] The preparation method of the PBT composite material of the present invention comprises the following steps: mixing the components uniformly according to the proportion, and then extruding and granulating through a twin-screw extruder to obtain the PBT composite material, wherein the temperature of the first zone from the feed port to the die head of the twin-screw extruder is 200-230°C, the temperature of the second zone is 240-260°C, the temperature of the third zone is 235-255°C, the temperature of the fourth zone is 235-255°C, the temperature of the fifth zone is 235-255°C, the temperature of the sixth zone is 240-260°C, the temperature of the seventh zone is 240-260°C, the temperature of the eighth zone is 220-240°C, the temperature of the ninth zone is 220-240°C, the temperature of the tenth zone is 240-260°C, and the screw speed is 200-450 rpm.

[0027] The PBT composite material of the present invention is used for preparing laser-welded thin-wall flame-retardant parts with a thickness of 2 mm or less.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] Phosphazene halogen-free flame retardant synergists contain phosphorus-nitrogen double bonds, which can effectively stabilize diethyl aluminum hypophosphite. On the one hand, the present invention uses a composite flame retardant of diethyl aluminum hypophosphite / phosphazene halogen-free flame retardant synergists, which not only has good flame retardancy, but also has less absorption of 980nm laser. On the other hand, by using polyethylene glycol with a specific average molecular weight and an epoxy chain extender, the crystallization ability of PBT can be enhanced, the thickness of the wafer can be reduced, thereby effectively reducing laser absorption, and the fluidity can be improved to achieve thin-wall flame retardancy. The PBT composite material of the present invention has the advantages of good thin-wall flame retardancy and is suitable for laser welding. Implementation

[0030] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0031] The sources of raw materials used in the present invention are as follows:

[0032] PBT-A: PBT GX110, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 0.6 dL / g;

[0033] PBT-B: PBT GX112, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 0.8 dL / g;

[0034] PBT-C: PBT GX121, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 1.0 dL / g

[0035] PBT-D: PBT GL236, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 1.2 dL / g;

[0036] Diethylaluminum hypophosphite: Exolit OP1230, Clariant, Germany;

[0037] Aluminum hypophosphite: M-116, Shanghai Meilaipo Chemical Material Technology Co., Ltd.;

[0038] Hexaphenoxycyclotriphosphazene, HPCTP, Foshan Hongda Dante Chemical Co., Ltd.; solid phosphate flame retardant: Daihachi Chemical Industry Co., Ltd., PX-200;

[0039] Melamine polyphosphate: BUDIT 3141, Budenheim, Germany;

[0040] Polyethylene glycol A: average molecular weight 1000, Hai'an Petrochemical Plant, Jiangsu Province;

[0041] Polyethylene glycol B: average molecular weight 2000, Hai'an Petrochemical Plant, Jiangsu Province;

[0042] Polyethylene glycol C: average molecular weight 3000, Hai'an Petrochemical Plant, Jiangsu Province;

[0043] Polyethylene glycol D: average molecular weight 4000, from Haian Petrochemical Plant, Jiangsu Province;

[0044] Polyethylene glycol E: average molecular weight 800, Hai'an Petrochemical Plant, Jiangsu Province;

[0045] Polyethylene glycol F: average molecular weight 6000, Hai'an Petrochemical Plant, Jiangsu Province;

[0046] Epoxy chain extender A: bisphenol A diglycidyl ether, Guodu Chemical Co., Ltd., YD-019;

[0047] Epoxy chain extender B: 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, Wuhan Chengtian Fine Chemical Co., Ltd., CT0961;

[0048] Pentaerythritol phosphate: Hubei Xinmingtai Chemical Co., Ltd.;

[0049] Embodiment and comparative example Preparation method of PBT composite material: According to the ratio, the components are mixed uniformly, and then extruded and granulated by a twin-screw extruder to obtain a PBT composite material, wherein the temperature of the first zone of the twin-screw extruder from the feed port to the die is 200-230°C, the temperature of the second zone is 240-260°C, the temperature of the third zone is 235-255°C, the temperature of the fourth zone is 235-255°C, the temperature of the fifth zone is 235-255°C, the temperature of the sixth zone is 240-260°C, the temperature of the seventh zone is 240-260°C, the temperature of the eighth zone is 220-240°C, the temperature of the ninth zone is 220-240°C, the temperature of the tenth zone is 240-260°C, and the screw speed is 200-450 rpm.

[0050] Various test methods:

[0051] (1) Flame retardancy: UL94-2018, vertical burning strip, strip size 127*13*0.8mm and 127*13*0.4mm.

[0052] (2) Fluidity test: The spiral length of each sample was injection molded at a temperature of 260°C and a pressure of 80 MPa. 51 films were continuously injected and the spiral length of the last mold product was tested. The longer the length, the better the fluidity of the product.

[0053] (3) Laser transmittance test: The sample size is 100*100*2.0mm, and the wavelength range of the laser transmittance test is 900-1150nm, with a focus on 980nm laser transmittance, because the wavelength of laser welding is around 980nm.

[0054] Table 1: Content of each component (parts by weight) and test results of PBT composite materials in Examples 1-7

[0055] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 PBT-A 50 PBT-B 50 PBT-C 50 50 50 50 PBT-D 50 Diethylaluminum hypophosphite 10 8 12 16 12 12 12 Hexaphenoxycyclotriphosphazene 4 7 5 3 5 5 5 Polyethylene glycol A 2 1 3 4 Polyethylene glycol B 3 Polyethylene glycol C 3 Polyethylene glycol D 3 Epoxy chain extender A 0.1 0.2 0.15 0.3 0.15 0.15 0.15 Flame retardant (0.8mm) V-0 V-0 V-0 V-0 V-0 V-0 V-0 Flame retardant (0.4mm) V-1 V-1 V-0 V-0 V-0 V-0 V-0 Helix length, mm 250 245 258 263 263 259 251 Laser transmittance, % 25.2 25.4 27.1 29.4 27.6 27.5 27.3

[0056] It can be seen from the examples that the PBT composite material of the present invention has excellent thin-wall flame retardancy, melt fluidity and a laser transmittance of ≥25.2%.

[0057] It can be seen from Examples 3 / 5-7 that the average molecular weight of polyethylene glycol is preferably 2000-3000.

[0058] Table 2: Content of each component (parts by weight) and test results of PBT composite materials in Examples 8-11

[0059] Example 8 Example 9 Example 10 PBT-A 50 50 50 Diethylaluminum hypophosphite 10 10 10 Hexaphenoxycyclotriphosphazene 4 4 4 Polyethylene glycol A 2 2 2 Epoxy chain extender A 0.1 0.1 Epoxy chain extender B 0.1 Pentaerythritol phosphate 0.1 0.5 Flame retardant (0.8mm) V-0 V-0 V-0 Flame retardant (0.4mm) V-0 V-0 V-0 Helix length, mm 256 267 285 Laser transmittance, % 27.2 27.4 28.1

[0060] It can be seen from Examples 1 / 9-10 that adding pentaerythritol phosphate can further improve flame retardancy, melt fluidity and laser transmittance.

[0061] Table 3: Content of each component (parts by weight) and test results of PBT composite materials in Examples 11-14

[0062] Embodiment 11 Example 12 Embodiment 13 Embodiment 14 PBT-C 50 50 50 50 Diethylaluminum hypophosphite 12 12 12 12 Hexaphenoxycyclotriphosphazene 5 5 5 5 Polyethylene glycol A 1 1.5 3.5 4 Epoxy chain extender A 0.3 0.15 0.25 0.1 Flame retardant (0.8mm) V-0 V-0 V-0 V-0 Flame retardant (0.4mm) V-1 V-0 V-0 V-1 Helix length, mm 250 256 255 249 Laser transmittance, % 25.7 26.8 26.4 25.7

[0063] It can be seen from Examples 3 / 11-14 that the preferred component content has better fluidity, improved thin-wall flame retardancy, and higher laser transmittance.

[0064] Table 4: Content of each component (parts by weight) and test results of comparative PBT composite materials

[0065] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 PBT-C 50 50 50 50 50 50 50 Diethylaluminum hypophosphite 12 12 12 12 12 12 Aluminum Hypophosphite 12 Hexaphenoxycyclotriphosphazene 5 5 5 5 5 Solid phosphate flame retardant 5 Melamine polyphosphate 5 Polyethylene glycol A 3 3 3 3 3 Polyethylene glycol E 3 Polyethylene glycol F 3 Epoxy chain extender A 0.15 0.15 0.03 0.4 0.15 0.15 0.15 Flame retardant (0.8mm) V-0 V-0 V-0 V-0 V-2 V-2 V-2 Flame retardant (0.4mm) V-1 V-1 V-1 V-1 HB HB HB Helix length, mm 258 243 253 239 224 234 225 Laser transmittance, % 22.4 20.3 21.1 22.4 7.8 15.4 12.8

[0066] It can be seen from Comparative Examples 1 / 2 that the average molecular weight of polyethylene glycol not only affects the crystallization ability and laser transmittance of PBT, but also significantly affects the melt fluidity. If the average molecular weight of polyethylene glycol is not within the scope of the present invention, good thin-wall flame retardancy, melt fluidity, and high laser transmittance cannot be achieved simultaneously.

[0067] It can be seen from Comparative Examples 3 / 4 that if the content of the epoxy chain extender is too low, the laser transmittance is low; if the content of the epoxy chain extender is too high, the melt fluidity will be significantly affected.

[0068] It can be seen from Comparative Example 5 that the laser transmittance of aluminum hypophosphite is low.

[0069] It can be seen from Comparative Examples 6 / 7 that the use of conventional solid phosphate flame retardant or melamine polyphosphate not only has poor flame retardancy but also low laser transmittance.

Claims

1. A PBT composite material, characterized in that: According to parts by weight, it includes the following components: 50 parts of PBT resin; 8-16 parts of diethyl aluminum hypophosphite; 3-7 parts of phosphazene halogen-free flame retardant synergist; 1-4 parts of polyethylene glycol; Epoxy chain extender 0.1-0.3 parts; The average molecular weight of the polyethylene glycol is 1000-4000; The phosphazene halogen-free flame retardant synergist is selected from at least one of hexaphenoxy cyclotriphosphazene, monocyanophenoxypentaphenoxy cyclotriphosphazene, dicyanophenoxytetraphenoxy cyclotriphosphazene and tricyanophenoxytriphenoxy cyclotriphosphazene; The epoxy chain extender is selected from at least one of bisphenol A diglycidyl ether and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate.

2. The PBT composite material according to claim 1, characterized in that: According to parts by weight, it includes the following components: 50 parts of PBT resin; 8-16 parts of diethyl aluminum hypophosphite; 3-7 parts of phosphazene halogen-free flame retardant synergist; 1.5-3.5 parts of polyethylene glycol; Epoxy chain extender 0.15-0.25 parts.

3. The PBT composite material according to claim 1, characterized in that: The average molecular weight of the polyethylene glycol is 2000-3000.

4. The PBT composite material according to claim 1, characterized in that The intrinsic viscosity of the PBT resin is in the range of 0.6-1.2 dL / g, and the test condition is 25°C.

5. The PBT composite material according to claim 1, characterized in that: By weight, 0-1.5 parts of pentaerythritol phosphate are also included.

6. The method for preparing the PBT composite material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing the components uniformly according to the proportion, and then extruding and granulating the components through a twin-screw extruder to obtain a PBT composite material, wherein the temperature of the first zone from the feeding port to the die head of the twin-screw extruder is 200-230°C, the temperature of the second zone is 240-260°C, the temperature of the third zone is 235-255°C, the temperature of the fourth zone is 235-255°C, the temperature of the fifth zone is 235-255°C, the temperature of the sixth zone is 240-260°C, the temperature of the seventh zone is 240-260°C, the temperature of the eighth zone is 220-240°C, the temperature of the ninth zone is 220-240°C, the temperature of the tenth zone is 240-260°C, and the screw speed is 200-450 rpm.

7. Application of the PBT composite material according to any one of claims 1 to 5, characterized in that: Used to prepare thin-walled flame-retardant parts for laser welding.