Two-component primer for polyurethane-lined composite metal pipes and its preparation method and application
Through the use of double-liquid primer, the problem of unsolid bonding of polyurethane-lined composite metal pipes is solved, and good bonding between polyurethane and the inner wall of metal pipes is achieved within the range of room temperature to 100℃ is achieved, which improves service life and Security.
Patent Information
- Application Number
- CN202310349031.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During use, polyurethane-lined composite metal pipes are often affected by the poor bonding between the inner wall of the pipe, which leads to the service life and safety. Especially in large pipes, it is difficult to throw sand and heat due to size reasons, resulting in peeling of the lining. Frequent situations occur.
Using a two-liquid primer, the preparation method of components A and B includes polyetherester diol with 2,4-toluene diisocyanate and 4,4'-diamino-3,3' -The combination of dichlorodiphenylmethane forms a liquid primer rich in highly reactive isocyanate groups, which is used to combine with the Camlock adhesive within a room temperature to 100°C to achieve good bonding between the polyurethane and the inner wall of the metal pipe.
The primer has good bonding performance and compatibility, and can achieve good bonding between polyurethane and the inner wall of the metal pipe at room temperature to 100°C. It is easy to use and stable storage, avoids the problem of lining peeling and extends the pipe service life and safety.
Smart Images

Figure CN116515378B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a primer for a polyurethane lined composite metal pipeline, in particular to a two-liquid primer for a polyurethane lined composite metal pipeline, a preparation method and an application thereof. Background Art
[0002] Polyurethane lined composite metal pipes have the advantages of high bearing capacity, good wear resistance, corrosion resistance, chemical resistance, and long service life. They are widely used in the transportation of various media such as sand, water, tailings, chemicals, salt lake brine, etc. The bonding strength between polyurethane and the inner surface of the metal pipe is the main factor affecting the service life and safety of this type of composite structure pipe. Chemlok is a commonly used adhesive between polyurethane and metal. In order to obtain a good bonding effect, the metal surface needs to be sandblasted to obtain sufficient roughness, and the surface temperature needs to reach above 90°C. Due to the large size and heavy weight of the metal pipe, it is difficult to sandblast the inner surface; at the same time, the amount of polyurethane lining is large, and the pouring time is relatively long. During the pouring and initial curing of polyurethane, the pipe needs to maintain high-speed rotation, which is difficult to heat and the inner surface temperature of the pipe is difficult to guarantee. Therefore, during the use of this type of pipe, the inner lining polyurethane and the inner wall of the pipe often peel off, affecting the service life and safety of the pipe. Summary of the invention
[0003] In order to overcome the shortcoming of weak adhesion between polyurethane and the inner surface of the pipe during the preparation of polyurethane lined composite metal pipes in the prior art, the purpose of the present invention is to provide a two-liquid primer for polyurethane lined composite metal pipes, which has good bonding performance and is easy to use. The lining polyurethane can be poured at a temperature of room temperature to 100°C to achieve good adhesion between the polyurethane and the inner wall of the metal pipe.
[0004] Another object of the present invention is to provide the above-mentioned two-component primer for polyurethane-lined composite metal pipes.
[0005] Another object of the present invention is to provide an application of the above-mentioned two-component primer for polyurethane-lined composite metal pipes.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A method for preparing a two-liquid primer for a polyurethane-lined composite metal pipe comprises the following steps:
[0008] Preparation of component A: adding polyether ester diol to a reaction kettle, heating to 100-120° C., evacuating to a residual pressure of less than 500 Pa, and keeping warm for 1.5-2 hours. When the water content of the polyether ester diol is less than 0.05%, adding a dehydrating agent and stirring for 15-30 minutes; then cooling the polyether ester diol to 50-60° C., adding 2,4-toluene diisocyanate, gradually heating to 80-85° C. and reacting for 1-2 hours, then adding ethyl acetate and stirring for 5-15 minutes to obtain component A;
[0009] Wherein, the molar ratio of 2,4-toluene diisocyanate to polyether ester diol is (4-6):1; the mass of the dehydrating agent is 0.5-1.5% of the mass of the polyether ester diol;
[0010] Wherein, the dehydrating agent is a dehydrating agent after heat treatment, and the heat treatment is specifically:
[0011] Heat treatment at 500-600°C for 2-3 hours;
[0012] Preparation of component B: 4,4'-diamino-3,3'-dichlorodiphenylmethane is placed in a container, heated to 115-125°C, vacuumed for 1-2 hours to remove water, then cyclohexanone is added, stirred for 15-30 minutes, to obtain component B;
[0013] The mass ratio of cyclohexanone to 4,4'-diamino-3,3'-dichlorodiphenylmethane is (1.9-2.5):1.
[0014] Preferably, the chain extension coefficient of the 4,4'-diamino-3,3'-dichlorodiphenylmethane is 0.8 to 0.9.
[0015] Preferably, the mass ratio of component A to component B is 100:(50-80).
[0016] Preferably, the dehydrating agent is zeolite molecular sieve.
[0017] Preferably, the average molecular weight of the polyether ester diol is 1500-3500.
[0018] Preferably, the solid content of component A is 75-80%.
[0019] Preferably, the solid content of component B is 25-35%.
[0020] Preferably, the solid content of component A is 76-78%.
[0021] Preferably, in the component A, the mass percentage of isocyanate groups is between 7% and 8%.
[0022] A two-liquid primer for polyurethane-lined composite metal pipes, comprising component A and component B;
[0023] The component A comprises polyether ester diol / 2,4-toluene diisocyanate polyurethane prepolymer, ethyl acetate, and zeolite molecular sieve;
[0024] The polyether ester diol / 2,4-toluene diisocyanate polyurethane prepolymer is prepared by prepolymerization of polyether ester diol and 2,4-toluene diisocyanate polyurethane; the molar ratio of 2,4-toluene diisocyanate to polyether ester diol is (4-6):1;
[0025] The component B includes 4,4'-diamino-3,3'-dichlorodiphenylmethane and cyclohexanone;
[0026] The mass ratio of component A to component B is 100:(50-90).
[0027] The application of the two-component primer for polyurethane lined composite metal pipe is used to prepare polyurethane lined composite metal pipe, which specifically includes the following steps:
[0028] After cleaning, derusting and polishing the inside of the metal pipe, apply a layer of Chemlock diluent by brushing, put it in a drying oven, heat it at 100-120°C for 30-60 minutes, apply the two-liquid primer for polyurethane lined composite metal pipe by brushing, and keep it at 100-120°C for 30-60 minutes;
[0029] The polyurethane lining is poured at a temperature between room temperature and 100°C to obtain a polyurethane lined composite metal pipe.
[0030] Preferably, the Chemlok is Chemlok218, Chemlok219 or Chemlok219 / 213.
[0031] Preferably, the lining polyurethane is polyether type or polyester type.
[0032] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0033] (1) The two-component primer for polyurethane-lined composite metal pipes of the present invention is rich in highly active isocyanate groups, can form chemical bonds with Chemlock when used, and has good bonding properties; and the urethane and urea groups generated by the two-component primer after curing have good compatibility with the lining polyurethane, further improving the bonding properties.
[0034] (2) The two-component primer for polyurethane-lined composite metal pipes of the present invention is prepared from polyether-ester diols and has good affinity with both polyether-type and polyester-type polyurethanes.
[0035] (3) The two-component primer for polyurethane-lined composite metal pipes of the present invention has component A and component B both in liquid form and with low viscosity. It can be applied to the inner wall of the pipe by brushing, and is easy to use.
[0036] (4) The two-component primer for polyurethane-lined composite metal pipes of the present invention is added with a dehydrating agent, so that the primer component A has good storage stability.
[0037] (5) The polyurethane-lined composite metal pipe is prepared by using the two-component primer for the polyurethane-lined composite metal pipe of the present invention. The lining polyurethane is poured at a temperature between room temperature and 100° C., which can achieve good adhesion between the polyurethane and the inner wall of the metal pipe. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The peeling curves of the primers prepared in Examples 1-3 and Comparative Examples 1-3 are shown. DETAILED DESCRIPTION
[0039] The present invention will be further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0040] Example 1
[0041] The preparation method of the two-component primer for the polyurethane lined composite metal pipe of this embodiment comprises the following steps:
[0042] (1) Preparation of component A
[0043] Weigh 100 parts by weight of polyether ester diol (CAPA7201) with an average molecular weight of 2000, add it to a reactor, heat it to 100-120°C, evacuate it to a residual pressure of less than 500Pa, and keep it warm for 2 hours. When the water content of the polyether ester diol is less than 0.05%, add 0.5 parts by weight of heat-treated dehydrating agent ZSM-5 (Zeochem Company) and stir it for 15 minutes. Then cool the polyether ester diol to 50-60°C, add 34.92 parts by weight of 2,4-toluene diisocyanate (Desmodur T100), and the molar ratio of 2,4-toluene diisocyanate to polyether ester diol is 4:1. Gradually heat it to 80-85°C and react for 2 hours, add 40.5 parts by weight of ethyl acetate (analytical grade), stir it for 5 minutes, and obtain component A. The solid content of component A is 76.9%, and the mass percentage of isocyanate group is 7.18%.
[0044] (2) Preparation of component B
[0045] 100 parts by weight of 4,4'-diamino-3,3'-dichlorodiphenylmethane (Suzhou Xiangyuan New Materials Co., Ltd.) was weighed, heated to 115-125° C., vacuumed for 1 hour to remove water, 200 parts by weight of cyclohexanone (analytical grade) was added, and stirred for 15 minutes to completely dissolve 4,4'-diamino-3,3'-dichlorodiphenylmethane to obtain component B. The solid content of component B was 33.3%.
[0046] (3) Preparation of two-component primer
[0047] Weigh 100 parts by weight of component A and 54.8 parts by weight of component B and mix them evenly. At this time, the chain extension coefficient of 4,4'-diamino-3,3'-dichlorodiphenylmethane is 0.8. The viscosity of the two-component primer is 350±30 MPa·s.
[0048] The use of the two-component primer for the polyurethane lined composite metal pipe of this embodiment to prepare the polyurethane lined composite metal pipe includes the following steps:
[0049] After cleaning, derusting and polishing, the inner wall of the metal pipe is brushed with a layer of Chemlok 218 dilution, which is prepared by mixing Chemlok 218 with isopropyl alcohol (analytical grade) at a mass ratio of 1:1. After coating with the Chemlok 218 dilution, the pipe is placed in a drying oven and kept at 100°C for 60 minutes, and then the two-component primer prepared in step (3) is brushed on and kept at 100°C for 60 minutes.
[0050] The pipe treated in the above steps is lined with polyurethane poured at 60°C.
[0051] Example 2
[0052] The preparation method of the two-component primer for the polyurethane lined composite metal pipe of this embodiment comprises the following steps:
[0053] (1) Preparation of component A
[0054] Weigh 100 parts by weight of polyether ester diol (self-made) with an average molecular weight of 2500, add it to the reactor, heat it to 100-120°C, evacuate it to a residual pressure of less than 500Pa, keep it warm for 2 hours, and when the water content of the polyether ester diol is less than 0.05%, add 1.0 parts by weight of heat-treated dehydrating agent Z1250 (Ningbo Jiahe New Material Technology Co., Ltd.) and stir it for 20 minutes. Then cool the polyether ester diol to 50-60°C, add 34.92 parts by weight of 2,4-toluene diisocyanate (Desmodur T100), and the molar ratio of 2,4-toluene diisocyanate to polyether ester diol is 5:1. Gradually heat it to 80-85°C and react for 2 hours, add 40.5 parts by weight of ethyl acetate (analytical grade), stir it for 10 minutes, and obtain component A. The solid content of component A is 76.9%, and the mass percentage of isocyanate group is 7.66%.
[0055] (2) Preparation of component B
[0056] 100 parts by weight of 4,4'-diamino-3,3'-dichlorodiphenylmethane (Suzhou Xiangyuan New Materials Co., Ltd.) was weighed, heated to 115-125° C., vacuumed for 1.5 hours to remove water, 230 parts by weight of cyclohexanone (analytical grade) was added, and stirred for 20 minutes to completely dissolve 4,4'-diamino-3,3'-dichlorodiphenylmethane to obtain component B. The solid content of component B was 30.3%.
[0057] (3) Preparation of two-component primer
[0058] Weigh 100 parts by weight of component A and 68.3 parts by weight of component B and mix them evenly. At this time, the chain extension coefficient of 4,4'-diamino-3,3'-dichlorodiphenylmethane is 0.85. The viscosity of the two-component primer is 230±30 MPa·s.
[0059] The use of the two-component primer for the polyurethane lined composite metal pipe of this embodiment to prepare the polyurethane lined composite metal pipe includes the following steps:
[0060] After cleaning, derusting and polishing, the inner wall of the pipeline is brushed with a layer of Chemlok 219 dilution, which is prepared by mixing Chemlok 219 with ethanol (analytical grade) at a mass ratio of 1:1. After coating with the Chemlok 219 dilution, the pipeline is placed in a drying oven and kept at 110°C for 45 minutes, and then brushed with the two-component primer prepared in step (3) and kept at 110°C for 45 minutes.
[0061] The pipe treated in the above steps is lined with polyurethane poured at 60°C.
[0062] Example 3
[0063] A two-liquid primer for a polyurethane-lined composite metal pipe and a preparation method thereof, comprising the following steps:
[0064] (1) Preparation of component A
[0065] Weigh 100 parts by weight of polyether ester diol (self-made) with an average molecular weight of 3000, add it to the reactor, heat it to 100-120°C, evacuate it to a residual pressure of less than 500Pa, keep it warm for 2 hours, and when the water content of the polyether ester diol is less than 0.05%, add 1.5 parts by weight of heat-treated dehydrating agent 13X molecular sieve (Tianjin Zhengyuan Haoye Chemical Co., Ltd.), and stir for 30 minutes. Then cool the polyether ester diol to 50-60°C, add 34.92 parts by weight of 2,4-toluene diisocyanate (Desmodur T100), and the molar ratio of 2,4-toluene diisocyanate to polyether ester diol is 6:1. Gradually heat it to 80-85°C and react for 2 hours, add 40.5 parts by weight of ethyl acetate (analytical grade), stir for 15 minutes, and obtain component A. The solid content of component A is 76.9%, and the mass percentage of isocyanate group is 8.0%.
[0066] (2) Preparation of component B
[0067] 100 parts by weight of 4,4'-diamino-3,3'-dichlorodiphenylmethane (Suzhou Xiangyuan New Materials Co., Ltd.) was weighed, heated to 115-125°C, vacuumed for 1.5 hours to remove water, 250 parts by weight of cyclohexanone (analytical grade) was added, and stirred for 30 minutes to completely dissolve 4,4'-diamino-3,3'-dichlorodiphenylmethane to obtain component B. The solid content of component B was 28.6%.
[0068] (3) Preparation of two-component primer
[0069] Weigh 100 parts by weight of component A and 80 parts by weight of component B and mix them evenly. At this time, the chain extension coefficient of 4,4'-diamino-3,3'-dichlorodiphenylmethane is 0.9. The viscosity of the two-component primer is 180±30 MPa·s.
[0070] The use of the two-component primer for the polyurethane lined composite metal pipe of this embodiment to prepare the polyurethane lined composite metal pipe includes the following steps:
[0071] After cleaning, derusting and polishing the inner wall of the pipeline, a layer of Chemlok 219 dilution was brushed on the inner wall. The dilution was prepared by mixing Chemlok 219 with ethanol (analytical grade) in a mass ratio of 1:1. After standing at room temperature for 30 minutes, a layer of Chemlok 213 dilution was brushed on the inner wall. The dilution was prepared by mixing Chemlok 213 with ethylene glycol monomethyl ether (analytical grade) in a mass ratio of 1:1. After coating with Chemlok, the pipeline was placed in a drying oven and heated at 120°C for 30 minutes. The two-component primer prepared in step (3) was brushed on and kept at 120°C for 30 minutes.
[0072] The pipe treated in the above steps is lined with polyurethane poured at room temperature.
[0073] Comparative Example 1
[0074] After cleaning, rust removal and polishing, the inner wall of the pipe is brushed with a layer of Chemlok 218 dilution, which is prepared by mixing Chemlok 218 with isopropanol (analytical grade) at a mass ratio of 1:1. After coating with Chemlok 218 dilution, the pipe is placed in a drying oven and heated at 100°C for 60 minutes.
[0075] The pipe treated in the above steps is lined with polyurethane poured at 100°C.
[0076] Comparative Example 2
[0077] After cleaning, rust removal and polishing, the inner wall of the pipe is brushed with a layer of Chemlok 218 dilution, which is prepared by mixing Chemlok 218 with isopropanol (analytical grade) at a mass ratio of 1:1. After coating with Chemlok 218 dilution, the pipe is placed in a drying oven and heated at 100°C for 60 minutes.
[0078] The pipe treated in the above steps is lined with polyurethane poured at 60°C.
[0079] Comparative Example 3
[0080] After cleaning, rust removal and polishing, the inner wall of the pipe is brushed with a layer of Chemlok 218 dilution, which is prepared by mixing Chemlok 218 with isopropanol (analytical grade) at a mass ratio of 1:1. After coating with Chemlok 218 dilution, the pipe is placed in a drying oven and heated at 100°C for 60 minutes.
[0081] The pipe treated in the above steps is lined with polyurethane poured at room temperature.
[0082] The specific effects of the two-component primers prepared in Examples 1-3 and Comparative Examples 1-3 are shown in Table 1.
[0083] Table 1: Effect of two-component primer on polyurethane / metal bonding performance*
[0084]
[0085] * Table 1 shows the bonding strength of polyurethane / iron sheet bonding strips. The preparation method of the bonding strips is as follows: 3mm thick iron sheet, cut into 25×200mm size, clean the surface, remove rust, apply adhesive according to the treatment process of the inner wall of the pipeline, and then pour the cast polyurethane onto the surface of the iron sheet, the thickness of the polyurethane is 3mm. According to GB / T 15254-2014 standard, the strips are subjected to T-type peeling test, and the tensile speed is 50mm / min.
[0086] The peeling curves of the primers prepared in Examples 1-3 and Comparative Examples 1-3 are as follows: Figure 1 shown.
[0087] From Table 1 and Figure 1 It can be seen that the two-liquid primer prepared by the present invention can achieve good adhesion with the cast polyurethane when the metal surface temperature is in the range of room temperature to 100°C.
[0088] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A two-component primer for polyurethane lined composite metal pipes, characterized in that: Comprising component A and component B; The component A comprises polyether ester diol / 2,4-toluene diisocyanate polyurethane prepolymer, ethyl acetate, and zeolite molecular sieve; The polyether ester diol / 2,4-toluene diisocyanate polyurethane prepolymer is prepared by prepolymerization of polyether ester diol and 2,4-toluene diisocyanate polyurethane; the molar ratio of 2,4-toluene diisocyanate to polyether ester diol is (4-6):1; The component B includes 4,4'-diamino-3,3'-dichlorodiphenylmethane and cyclohexanone; The mass ratio of component A to component B is 100:(50-90); the chain extension coefficient of 4,4'-diamino-3,3'-dichlorodiphenylmethane is 0.8-0.9; When the two-liquid primer is used for preparing the polyurethane lined composite metal pipe, the steps are specifically as follows: After cleaning, derusting and polishing the inside of the metal pipe, apply a layer of Chemlock diluent by brushing, put it in a drying oven, heat it at 100-120°C for 30-60 minutes, apply the two-liquid primer for polyurethane lined composite metal pipe by brushing, and keep it at 100-120°C for 30-60 minutes; The polyurethane lining is poured at a temperature between room temperature and 60°C to obtain a polyurethane lined composite metal pipe.
2. The two-component primer for polyurethane-lined composite metal pipe according to claim 1, characterized in that: The Chemlok is Chemlok218, Chemlok219 or Chemlok219 / 213.
3. The method for preparing the two-component primer for polyurethane-lined composite metal pipe according to claim 1 or 2, characterized in that: The following steps are involved: Preparation of component A: add polyether ester diol to a reaction kettle, heat to 100-120°C, evacuate to a residual pressure of less than 500Pa, and keep warm for 1.5-2 hours. When the water content of the polyether ester diol is less than 0.05%, add zeolite molecular sieve and stir for 15-30 minutes; then cool the polyether ester diol to 50-60°C, add 2,4-toluene diisocyanate, heat to 80-85°C, react for 1-2 hours, add ethyl acetate, and stir for 5-15 minutes to obtain component A; Wherein, the zeolite molecular sieve is a zeolite molecular sieve that has been heat-treated, and the heat treatment is specifically: Heat treatment at 500-600°C for 2-3 hours; Preparation of component B: 4,4'-diamino-3,3'-dichlorodiphenylmethane is placed in a container, heated to 115-125°C, vacuumed for 1-2 hours to remove water, then cyclohexanone is added, stirred for 15-30 minutes, to obtain component B; Among them, the mass ratio of cyclohexanone to 4,4'-diamino-3,3'-dichlorodiphenylmethane is (1.9-2.5):
1.
4. The method for preparing a two-component primer for a polyurethane-lined composite metal pipe according to claim 3, characterized in that: The average molecular weight of the polyether ester diol is 1500-3500.
5. The method for preparing a two-component primer for a polyurethane-lined composite metal pipe according to claim 3, characterized in that: The solid content of component A is 75-80%.
6. The method for preparing a two-component primer for a polyurethane-lined composite metal pipe according to claim 3, characterized in that: The solid content of component B is 25-35%.