A multiple annealing process suitable for Ti6242 alloy blades
Through multiple annealing treatment processes, including multi-stage heat treatment and argon or oxygen atmosphere protection, combined with polishing and polishing treatment, the problems of high internal stress and poor fatigue performance of the Ti6242 alloy blades are solved, which significantly improves the fatigue performance of the blades and reduces the internal stress. .
Patent Information
- Application Number
- CN202310599231.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-05-25
AI Technical Summary
Ti6242 alloy blades are subject to high internal stress and uneven distribution due to complex deformation during thermal processing, and are prone to abnormal failure in complex environments such as high temperature, cyclic loads and impacts.
Multiple annealing treatment process is adopted, including first heat treatment below the α/β phase transition point, second heat treatment at 550°C to 650°C, and third heat treatment at 490°C to 510°C, combined with argon or oxygen Atmosphere protection, finally polished to remove the oxide layer and retain the permeable oxygen layer.
It effectively reduces the stress in the blade, significantly improves fatigue performance, and forms a gradient oxygen permeability layer, improving the overall performance of the component.
Smart Images

Figure CN116516273B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heat treatment of titanium alloys, and in particular relates to a multiple annealing process suitable for Ti6242 alloy blades. Background Art
[0002] Ti6242 alloy is a near-α titanium alloy with a nominal composition of Ti-6A1-2Sn-4Zr-2Mo and a maximum operating temperature of 540°C. The alloying element Mo can increase room temperature and high temperature tensile strength and enhance stability;
[0003] Under the combined effect of A1, Sn and Zr, it can maintain long-term high-temperature strength and creep. Compared with other titanium alloys, the biggest advantage of this alloy is its good high-temperature resistance. This alloy not only combines strength, creep strength, toughness and thermal stability very well, but also has good welding performance. At present, Ti6242 alloy is mainly used to manufacture key components such as blades for aircraft engines. Since Ti6242 alloy blades often undergo complex deformation during hot working, the internal stress of the blades is high and unevenly distributed. In actual service environments, blades are usually in complex working conditions such as high temperatures, cyclic loads, and accidental impacts. Therefore, even under strict preparation process and quality control requirements and combined with comprehensive inspection and evaluation of each process step, some titanium alloy components still have abnormal failure events. Therefore, improvements are proposed for the annealing process of Ti6242 alloy blades. Summary of the invention
[0004] The purpose of the present invention is to provide a multiple annealing treatment process suitable for Ti6242 alloy blades. The process is simple to implement, can eliminate the internal stress of the Ti6242 alloy blades, and greatly improve the fatigue performance.
[0005] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] A multiple annealing process suitable for Ti6242 alloy blades, the specific process steps are:
[0007] Step 1: The forged Ti6242 alloy blade is placed in a heat treatment furnace at the α / β phase transition point T β The first heat treatment is carried out at 80℃~10℃, and after being heated thoroughly, it is kept warm for 1h~4h and then air-cooled;
[0008] Step 2: Perform the second heat treatment at 550℃~650℃, keep the temperature for 6~40h and then air cool;
[0009] Step 3: Perform the third heat treatment at 490℃~510℃, keep the temperature for 50h~200h and then air cool.
[0010] The multiple annealing treatment process suitable for Ti6242 alloy blades is preferably performed in the above step 1 and step 2 under the protection of argon gas.
[0011] The multiple annealing treatment process suitable for Ti6242 alloy blades is preferably carried out in the above step three in an oxygen atmosphere of 1 to 3 times the standard atmospheric pressure or in a mixed atmosphere with an oxygen concentration equivalent thereto.
[0012] The multiple annealing treatment process applicable to Ti6242 alloy blades has a preferred embodiment that, after annealing, the Ti6242 alloy blades are subjected to grinding and polishing to remove the oxide layer and retain the oxygen permeable layer.
[0013] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0014] 1. The process in this scheme is simple and easy to operate, has strong repeatability, low cost and significant effect;
[0015] 2. In this scheme, after multiple annealing treatments, the Ti6242 alloy blades have reduced the internal stress of the blades to the maximum extent, and a gradient oxygen permeation layer is formed on the surface of the blades, which greatly improves the fatigue performance of the components. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a microstructure photograph of the Ti6242 alloy blade near the surface in Example 1 of the present invention;
[0017] Figure 2 This is a photo of the internal microstructure of the Ti6242 alloy blade in Example 1 of the present invention. DETAILED DESCRIPTION
[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] The present invention will be further described below in conjunction with the embodiments.
[0020] Embodiment 1:
[0021] See also Figure 1-2As shown, the raw material used in this embodiment is a Ti6242 alloy with an alloy composition (wt%) of Ti-6.10Al-2.0Sn-4.0Zr-2.15Mo. After the Ti6242 alloy blade is subjected to complex deformation, it is subjected to T β After triple heat treatment at 15℃ for 2h below the phase transformation point and then air cooling, at 600℃ for 8h and then air cooling, and at 500℃ for 80h in an oxygen atmosphere of 1.5 times the standard atmospheric pressure and then air cooling, the microstructure is a dual-state microstructure with a volume fraction of the primary α phase of ~10%. The microstructure of the alloy is as follows Figure 2 After heat treatment, the blade surface is ground and polished using SiO 2 The polishing liquid completely removes the oxide layer on the surface of the sample, the surface thickness is removed by more than 50 μm, and the surface finish after processing is R = 0.1. Table 1 shows the fatigue limit of the Ti6242 alloy blade in Example 1. It can be seen that the Ti6242 alloy blade has excellent room temperature and high temperature fatigue properties after the multiple annealing treatment of the present invention.
[0022] Table 1 Fatigue properties of Ti6242 alloy blades in Example 1
[0023]
[0024]
[0025] In summary, after multiple annealing treatments, the Ti6242 alloy blades in the present invention reduce the internal stress of the blades to the maximum extent, and form a gradient oxygen permeation layer on the surface of the blades, so that the fatigue performance of the components is greatly improved. The process is simple and easy to operate, has strong repeatability, low cost, and significant effect.
[0026] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0027] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A multiple annealing process suitable for Ti6242 alloy blades, characterized in that: The specific process steps are: Step 1: The forged Ti6242 alloy blade is placed in a heat treatment furnace at the α / β phase transition point T β The first heat treatment is carried out at 80℃~10℃, and after being heated thoroughly, it is kept warm for 1h~4h and then air-cooled; Step 2: Perform the second heat treatment at 550℃~650℃, keep the temperature for 6h~40h and then air cool; Step 3: Perform the third heat treatment at 490℃~510℃, keep the temperature for 50h~200h and then air cool; In the above step three, the heat treatment is carried out in an oxygen atmosphere of 1 to 3 times the standard atmospheric pressure or in a mixed atmosphere with an oxygen concentration equivalent thereto.
2. A multiple annealing process suitable for Ti6242 alloy blades according to claim 1, characterized in that: In the above step 1 and step 2, the heat treatment is performed in an argon protective environment.
3. The multiple annealing process for Ti6242 alloy blades according to claim 1 is characterized in that: The Ti6242 alloy blade is subjected to grinding and polishing after annealing to remove the oxide layer and retain the oxygen permeable layer.