Antistatic polyester fiber and preparation method thereof

By using antistatic agents of modified carbon black and nanomontmorillonite in the preparation of polyester fibers, the electrostatic problem of polyester fibers is solved, its antistatic properties and mechanical strength are improved, and safety and resource recycling are ensured.

CN116516513BActive Publication Date: 2024-12-03CIXI JIANGNAN CHEM FIBER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310571079.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-20
Publication Date
2024-12-03
Estimated Expiration
2043-05-20

AI Technical Summary

Technical Problem

Static electricity is easily generated during the preparation of existing polyester fibers, which can easily cause dangers such as explosions and fires when worn, and have a low recycling rate.

Method used

Using antistatic agent composed of modified carbon black and nanomontmorillonite, the conductive carbon black is mixed with titanate coupling agent and dispersed uniformly in chitosan solution, and combined with nanomontmorillonite as a nucleation agent to promote The crystallization of polyester fiber improves its mechanical properties and anti-static properties.

Benefits of technology

The antistatic properties and mechanical strength of polyester fibers are significantly improved, safety is ensured and efficient recycling of polyester waste is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004238632340000071
    Figure BDA0004238632340000071
  • Figure BDA0004238632340000081
    Figure BDA0004238632340000081
Patent Text Reader

Abstract

The present invention relates to the field of polyester fiber preparation, and in particular to an antistatic polyester fiber and a preparation method thereof, which is mainly made of the following raw materials in parts by weight: 40-50 parts of PET masterbatch, 20-30 parts of PET bottle flakes, and 3-5 parts of antistatic agent; the antistatic agent is composed of modified carbon black and nano-montmorillonite in a mass ratio of (2-4): (1-3); the preparation method of the modified carbon black comprises the following steps: 1) mixing conductive carbon black with a titanate coupling agent to prepare an intermediate material; 2) uniformly dispersing the intermediate material prepared in step 1) in a chitosan solution, drying and crushing the intermediate material; the mass ratio of the conductive carbon black to chitosan is (2-3): (3-5). The present application has the advantage of improving the antistatic performance of the prepared polyester fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyester fiber preparation, in particular to an antistatic polyester fiber and a preparation method thereof. Background Art

[0002] Polyethylene terephthalate has the characteristics of high strength, chemical corrosion resistance, and good thermal stability. It is often used in the fields of synthetic fibers and food packaging. As a result, the amount of polyester waste generated each year is also very huge, but the recycling rate is very low, which causes a great waste of resources. One way to recycle polyester waste in existing production is to mix polyester waste with other raw materials, and then prepare polyethylene terephthalate fiber, referred to as polyester fiber, through a melt spinning process, and use it in clothing, blankets and other fields to achieve the recycling and utilization of waste polyester materials.

[0003] In the above-mentioned related technologies, the inventors believe that: the polyester fibers prepared from polyester waste products in the prior art are prone to generate static electricity. When the static electricity accumulates to a certain level, it will produce discharge, so that when the clothes made of polyester fibers are worn in certain occasions, they are prone to produce electric sparks due to static electricity, which in turn causes dangers such as explosions and fires. Therefore, it is necessary to improve the antistatic properties of the prepared polyester fibers. Summary of the invention

[0004] In order to improve the antistatic performance of the prepared polyester fiber, the present application provides an antistatic polyester fiber and a preparation method thereof.

[0005] In the first aspect, the present application provides an antistatic polyester fiber, which adopts the following technical solution:

[0006] An antistatic polyester fiber is mainly made of the following raw materials in parts by weight: 40-50 parts of PET masterbatch, 20-30 parts of PET bottle flakes, and 3-5 parts of antistatic agent; the antistatic agent is composed of modified carbon black and nano-montmorillonite in a mass ratio of (2-4): (1-3); the preparation method of the modified carbon black comprises the following steps:

[0007] 1) mixing conductive carbon black and titanate coupling agent to prepare an intermediate material;

[0008] 2) The intermediate material obtained in step 1) is uniformly dispersed in the chitosan solution, dried and crushed to obtain the conductive carbon black; the mass ratio of the conductive carbon black to the chitosan is (2-3):(3-5).

[0009] By adopting the above technical scheme, PET bottle flakes and other raw materials are mixed to prepare polyester fibers, thereby realizing the recycling of polyester waste. However, due to the strong hydrophobicity of polyester fibers, static electricity is easily generated, which affects the wearing experience. By adding an antistatic agent in the preparation process of polyester fibers, since the antistatic agent includes modified carbon black and nano-montmorillonite, and the conductive carbon black itself has a porous structure and adsorption performance, it can absorb moisture. At the same time, the conductive carbon black is dispersed in the polyester fibers to form a network-like conductive path, which disperses the charge on the surface of the prepared polyester fibers, thereby playing an antistatic role for the prepared polyester fibers. However, the compatibility of conductive carbon black with PET masterbatch and PET bottle flakes is general, and it is easy to detach during the subsequent washing process of the polyester fibers, affecting the conductivity of the polyester fibers. By mixing the conductive carbon black with a titanate coupling agent and immersing them in a chitosan solution, the titanium The acid ester coupling agent increases the dispersibility of the conductive carbon black in the chitosan solution, and the conductive carbon black is wrapped by chitosan. Since the structure of chitosan itself is similar to that of the polyethylene terephthalate molecule, chitosan is used to improve the compatibility of the conductive carbon black with the PET masterbatch and the PET bottle flakes according to the principle of similar compatibility, and at the same time improve the firmness of the conductive carbon black on the prepared polyester fiber; however, the addition of the conductive carbon black will affect the crystallization of the polyester fiber, and then affect the strength of the prepared polyester fiber. By compounding the nano-montmorillonite with the conductive carbon black, the addition of the nano-montmorillonite can be used as a nucleating agent to promote the crystallization of the polyester fiber, so that the generation rate of the crystal nucleus is accelerated, and the polyester fiber is promoted to form a relatively complete molecular chain structure, and the mechanical properties of the prepared antistatic polyester fiber are improved, so that the prepared polyester fiber not only has good antistatic properties, but also has good mechanical strength;

[0010] The mass ratio of conductive carbon black to chitosan is adjusted during the preparation process. Chitosan is used to wrap the conductive carbon black to improve compatibility, while too much chitosan is avoided and the thickness of the wrapping layer is too thick, which affects the antistatic effect of the prepared modified carbon black on polyester fibers.

[0011] Optionally, the nano-montmorillonite in the antistatic agent is immersed in a treatment liquid before use, and then taken out and dried; the treatment liquid includes a silane coupling agent.

[0012] By adopting the above technical scheme, the nano-montmorillonite is mixed and impregnated with a treatment liquid including a silane coupling agent. The silane coupling agent improves the dispersion performance of the nano-montmorillonite in other raw materials, so that the nano-montmorillonite promotes the crystallization performance of the polyester fiber more evenly; with the addition of the silane coupling agent, the silane coupling agent can effectively reduce the agglomeration of the nano-montmorillonite and improve the promotion effect of the nano-montmorillonite on the crystallization performance of the polyester fiber, so that the prepared polyester fiber has good antistatic effect and good mechanical properties; the silane coupling agent used in the present application is γ-aminopropyltriethoxysilane, and the treatment liquid used is a mixture of γ-aminopropyltriethoxysilane, anhydrous ethanol and water in a mass ratio of 1:5:10.

[0013] Optionally, the PET masterbatch is prepared by co-polymerization of sorbitol, ethylene glycol, terephthalic acid, isophthalic acid sulfonate and polyethylene glycol.

[0014] By adopting the above technical scheme, ethylene glycol and terephthalic acid are mixed and polymerized, and by introducing isophthalic acid sulfonate with a hydrophilic effect into the prepared PET masterbatch, the hydrophilicity of the prepared PET masterbatch is improved by combining with other raw materials, so that the prepared polyester fiber has hydrophilicity, can absorb moisture in the air and form a channel for leaking charges, so that the antistatic effect of the prepared polyester fiber is improved, and in combination with the use of an antistatic agent, the prepared polyester fiber has a better antistatic effect.

[0015] In a second aspect, the present application provides a method for preparing an antistatic polyester fiber;

[0016] A method for preparing antistatic polyester fiber mainly comprises the following steps:

[0017] S1: Mixing PET masterbatch, PET bottle flakes and antistatic agent together to prepare a mixed material;

[0018] S2: putting the mixed material obtained in step S1 into a melt spinning machine for spinning to prepare pre-finished fiber, and curling, oiling and cooling the pre-finished fiber.

[0019] By adopting the above technical scheme, PET masterbatch, PET bottle flakes and antistatic agent are first mixed and melted, and nano-montmorillonite is used as crystal nuclei to promote the crystallization rate of PET masterbatch and PET bottle flakes during the melting process, so that the generation rate of crystal nuclei is accelerated, and the improvement of the molecular chain structure of the prepared polyester fiber is promoted; and modified carbon black is added to make the conductive carbon black adhere to the inside of the polyester fiber to form a uniform conductive path, so that the prepared polyester fiber can disperse the surface charge, and the prepared polyester fiber has an antistatic effect; chitosan improves the compatibility of the conductive carbon black with other raw materials in the polyester fiber, and it is not easy to fall out during subsequent washing, thereby further improving the antistatic performance of the prepared polyester fiber.

[0020] Optionally, before curling and oiling the pre-finished fiber in step S2, the pre-finished fiber is first immersed in a silk solution, wherein the silk solution comprises silk fibroin and hexafluoroisopropanol, and the mass ratio of the silk fibroin to hexafluoroisopropanol is (7-10):(95-105).

[0021] By adopting the above technical scheme, the silk molecules contain a large number of hydrophilic groups such as -OH, -NH2, -COOH, etc. After the silk liquid is coated on the prepared polyester fiber product, the silk molecules with hydrophilic properties can adsorb water molecules in the air, so that the hydrophilicity of the prepared polyester fiber is improved, thereby reducing the surface resistivity of the prepared polyester fiber, accelerating the dissipation of charges, and improving the antistatic effect of the prepared polyester fiber.

[0022] Optionally, ethanol and tin chloride are further added to the silk fibroin solution, and the mass ratio of the ethanol, tin chloride and silk fibroin is (3-5):(2-3):(8-10).

[0023] By adopting the above technical scheme, ethanol as an organic solvent can make the silk film generated by the silk liquid beta-cured and then solidified, so that it is fixed on the pre-finished fiber. In combination with the tin ions in tin chloride, the tin ions can be adsorbed on the pre-finished fiber. At the same time, the tin ions can form chemical bonds with the coordination bonds in the side chains of the silk molecule and combine with the silk molecule, thereby improving the firmness of the silk liquid fixed on the polyester fiber, thereby improving the antistatic performance of the polyester fiber.

[0024] Optionally, before being immersed in the silk fibroin solution, the pre-finished fiber is first immersed in a lipase treatment solution, taken out, washed, and dried.

[0025] By adopting the above technical scheme, the prepared pre-finished fiber is placed in lipase for immersion treatment. Lipase is a type of hydrolase. The surface of the pre-finished fiber contains a large number of ester bonds, which can be hydrolyzed by lipase to produce polar hydroxyl and carboxyl groups, which are easier to combine with silk molecules in the silk solution later. At the same time, the surface of the polyester fiber treated with lipase is rough, which facilitates the penetration of silk fibroin molecular monomers when the silk solution is subsequently coated on the surface of the pre-finished fiber, thereby improving the firmness of the silk solution on the surface of the polyester fiber.

[0026] Optionally, the concentration of lipase in the lipase treatment solution is 0.3-0.8 g / L.

[0027] By adopting the above technical scheme, the concentration of lipase in the lipase treatment solution is adjusted. As the concentration of lipase increases, the hydrolysis effect on the polyester fiber is improved, so that the surface of the polyester fiber becomes rough, the subsequent contact area with the silk monomer is increased, and the firmness of the silk molecule on the surface of the polyester fiber is also improved; however, as the concentration of lipase increases, since the lipase does not hydrolyze all the ester bonds in the polyester fiber, continuing to increase the concentration of lipase will not continue to improve the hydrolysis effect on the polyester fiber, but will cause a waste of lipase, so it is necessary to control the concentration of lipase, so that the polyester fiber has a good hydrolysis effect while reducing the waste of lipase.

[0028] Optionally, the pH value of the lipase treatment solution is 6-10.

[0029] By adopting the above technical solution, the pH value of the lipase treatment solution is adjusted. When the pH value of the lipase treatment solution is low, the polyester fiber is not easily hydrolyzed by the lipase in an acidic environment. As the pH value increases, the hydrolysis effect of the lipase on the polyester fiber increases; however, when the pH value continues to increase, the hydroxyl content in the lipase treatment solution increases, causing the lipase to be irreversibly inactivated, thereby reducing the hydrolysis effect of the lipase on the polyester fiber. Therefore, by adjusting the pH value of the lipase treatment solution, the lipase treatment solution has a good hydrolysis effect on the pretreated fiber, thereby improving the antistatic properties of the subsequently prepared polyester fiber.

[0030] In summary, this application has the following beneficial effects:

[0031] The present application adds an antistatic agent composed of modified carbon black and nano-montmorillonite to the raw materials for preparing polyester fibers. The conductive carbon black itself has conductive properties and can form pathways on the surface of the polyester fibers, thereby improving the antistatic properties of the prepared polyester fibers. The compatibility of the conductive carbon black and the polyester fibers is improved by chitosan. Nano-montmorillonite is added as a nucleating agent to promote the improvement of the internal molecular chains of the polyester fibers, so that the polyester fibers have good antistatic effects and good mechanical strength. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments and comparative examples;

[0033] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0034] Preparation Example

[0035] Modified carbon black preparation example 1

[0036] The preparation method of modified carbon black in this preparation example comprises the following steps:

[0037] 1) Take a mixing barrel, put the conductive carbon black and the titanate coupling agent into the mixing barrel and mix them to prepare an intermediate material;

[0038] 2) adding the chitosan solution into the mixing barrel and mixing it evenly with the intermediate material to prepare a mixed solution, drying and crushing; the chitosan solution used is composed of chitosan and acetic acid solution in a mass ratio of 1:4; the mass concentration of acetic acid in the acetic acid solution used is 10%; the mass ratio of the conductive carbon black to the titanate coupling agent used is 4:0.3; the mass ratio of the conductive carbon black to the chitosan used is 2:5; the titanate coupling agent used in this application is triisostearoyl isopropyl titanate.

[0039] Modified carbon black preparation example 2

[0040] The difference between the preparation method of modified carbon black in this preparation example and that in the modified carbon black preparation example 1 is that the mass ratio of the conductive carbon black to chitosan used is 3:3.

[0041] Modified carbon black preparation example 3

[0042] The difference between the preparation method of modified carbon black in this preparation example and that in the modified carbon black preparation example 1 is that the mass ratio of the conductive carbon black to chitosan used is 2.5:4.

[0043] Example

[0044] Example 1

[0045] The raw materials for preparing the antistatic polyester fiber in this embodiment include the following raw materials in mass fractions: 40 kg of PET masterbatch, 20 kg of PET bottle flakes, and 3 kg of antistatic agent; the antistatic agent used is composed of modified carbon black and nano-montmorillonite in a mass ratio of 3:2; the modified carbon black used is prepared in Modified Carbon Black Preparation Example 1; the PET masterbatch used is prepared by co-condensation of sorbitol, ethylene glycol, terephthalic acid, isophthalic acid sulfonate and polyethylene glycol in a mass ratio of 5:2:8:2.5:3.5;

[0046] The preparation method of PET masterbatch in this embodiment comprises the following steps:

[0047] S1: Put the above proportions of sorbitol, ethylene glycol and terephthalic acid into an esterification reaction kettle for mixing to prepare a mixture, and then pressurize the mixture for esterification reaction at a temperature of 240° C. and a pressure of 0.3 MPa. When the esterification water output reaches 88%, the esterification reaction is terminated to prepare a pretreated material;

[0048] S2: adding the above proportions of isophthalic acid sulfonate and polyethylene glycol to the pretreated material prepared in step S1, and carrying out esterification reaction at normal pressure. When the esterification water output reaches 96%, the normal pressure esterification is completed; the pretreated material after the normal pressure esterification reaction is subjected to polycondensation at 260° C. and 60 kPa for 60 minutes, cooled and crushed to obtain the product; the isophthalic acid sulfonate used is sodium 5-sulfonate of isophthalic acid.

[0049] The preparation method of the antistatic polyester fiber in this embodiment comprises the following steps:

[0050] S1: After the PET bottle flakes are washed and dried, the PET masterbatch, PET bottle flakes and antistatic agent of the above mass are put into a stirring barrel and mixed evenly to prepare a mixture;

[0051] S2: The mixed material is placed in a melt spinning machine for melt extrusion spinning and stretching to prepare a pre-finished fiber, and the pre-finished fiber is curled, oiled and cooled; the spinning temperature is 258°C, the spinning rate is 800m / min; the stretching temperature is 60°C.

[0052] Example 2

[0053] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Example 1 in that the raw materials used in this embodiment are: 50 kg of PET masterbatch, 30 kg of PET bottle flakes, and 5 kg of antistatic agent.

[0054] The model of the PET masterbatch of the present embodiment is UL94-V0, and the manufacturer is Jin Zhicheng.

[0055] Example 3

[0056] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Example 1 in that the raw materials used in this embodiment are: 45 kg of PET masterbatch, 25 kg of PET bottle flakes, and 4 kg of antistatic agent; the nano-montmorillonite in the antistatic agent is immersed in the treatment liquid for 6 minutes before use, and then taken out and dried; the treatment liquid used is a mixture of γ-aminopropyltriethoxysilane, anhydrous ethanol and water in a mass ratio of 1:5:10.

[0057] Example 4

[0058] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Example 3 in that, before curling and oiling the pre-finished fiber in step S2, the pre-finished fiber is first immersed in a silk solution for 10 minutes and then taken out and dried; the silk solution used is composed of silk fibroin and hexafluoroisopropanol in a mass ratio of 8:100; the mass ratio of the silk fibroin used to the pre-finished fiber is 1:10.

[0059] Example 5

[0060] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Embodiment 4 in that ethanol and tin chloride are added to the silk fibroin solution before use, and the mass ratio of ethanol, tin chloride and silk fibroin is 3:2:8.

[0061] Example 6

[0062] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Embodiment 4 in that ethanol and tin chloride are added to the silk fibroin solution before use, and the mass ratio of ethanol, tin chloride and silk fibroin is 5:3:10.

[0063] Example 7

[0064] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Embodiment 4 in that ethanol and tin chloride are added to the silk fibroin solution before use, and the mass ratio of ethanol, tin chloride and silk fibroin is 4:2.5:9.

[0065] Example 8

[0066] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Example 7 in that before the pre-finished fiber is immersed in the silk solution, the pre-finished fiber is first placed in a lipase treatment solution and immersed for 20 minutes; the activity of the lipase in the lipase treatment solution used is 60U / mg, the mass concentration of the lipase in the lipase treatment solution is 0.3g / L, and the pH value of the lipase treatment solution used is 6.

[0067] Example 9

[0068] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Example 8 in that the activity of the lipase in the lipase treatment solution used is 60 U / mg, the concentration of the lipase in the lipase treatment solution is 0.8 g / L, and the pH value of the lipase treatment solution used is 10.

[0069] Example 10

[0070] The preparation method of the antistatic polyester fiber in this embodiment is different from that in Example 8 in that the activity of the lipase in the lipase treatment solution used is 60 U / mg, the concentration of the lipase in the lipase treatment solution is 0.5 g / L, and the pH value of the lipase treatment solution used is 8.5.

[0071] Embodiment 11

[0072] The method for preparing the antistatic polyester fiber in this embodiment is different from that in Example 10 in that the modified carbon black in the antistatic agent used in step S2 is prepared in Modified Carbon Black Preparation Example 2.

[0073] Example 12

[0074] The method for preparing the antistatic polyester fiber in this embodiment is different from that in Example 10 in that the modified carbon black in the antistatic agent used in step S2 is prepared in Modified Carbon Black Preparation Example 3.

[0075] Comparative Example

[0076] Comparative Example 1

[0077] The preparation method of the antistatic polyester fiber in this comparative example is different from that in Example 1 in that the antistatic agent used is composed of conductive carbon black and nano-montmorillonite in a mass ratio of 2:3.

[0078] Comparative Example 2

[0079] The preparation method of the antistatic polyester fiber in this comparative example is different from that in comparative example 1 in that the antistatic agent used in the raw materials of the antistatic polyester fiber in the preparation example is conductive carbon black.

[0080] Comparative Example 3

[0081] The preparation method of the antistatic polyester fiber in this comparative example is different from that in comparative example 1 in that the raw materials used for the antistatic polyester fiber in the preparation example do not include an antistatic agent.

[0082] Detection Methods

[0083] Antistatic fibers were prepared according to the preparation methods of antistatic polyester fibers in Examples 1-12 and Comparative Examples 1-3, and the prepared antistatic fibers were woven to prepare experimental fabrics.

[0084] The surface charge of the experimental fabric was tested according to GB / T12703.3-2009 "Test Method for Electrostatic Test of Textiles". The more charge, the worse the antistatic property; the less charge, the better the antistatic property. At the same time, the antistatic fibers prepared in Examples 1-12 and Comparative Examples 1-3 were tested for breaking strength using a fiber breaking strength tester, and the breaking strength of the fibers was recorded. The recorded data are shown in Table 1:

[0085] Table 1 Charge amount and breaking strength of antistatic fibers in Examples 1-12 and Comparative Examples 1-3

[0086]

[0087]

[0088] Combining Examples 1-7, Comparative Examples 1-3 and Table 1, it can be seen that by modifying the conductive carbon black, the compatibility and firmness of the conductive carbon black with the polyester fiber are improved through the encapsulation effect of chitosan; at the same time, nano-montmorillonite is added to compound with the modified carbon black, and the nano-montmorillonite promotes the improvement of the crystal form in the preparation process of the polyester fiber, so that the polyester fiber has a good antistatic effect and also improves the breaking strength of the prepared polyester fiber; before the conductive carbon black is mixed with the chitosan solution, the conductive carbon black is mixed with a titanate coupling agent, so that the conductive carbon black is better dispersed in the chitosan solution, which makes the conductive carbon black on the surface of the polyester fiber The distribution is more uniform, and the antistatic effect of the prepared polyester fiber is further improved; by immersing the pre-finished fiber in the silk solution before curling and oiling the pre-finished fiber, the hydrophilicity of the prepared polyester fiber is increased by the hydrophilic groups on the silk molecules, so that the surface of the polyester fiber forms a channel for leaking charges, thereby improving the antistatic effect of the prepared polyester fiber; at the same time, according to Examples 5-7, the addition amounts of ethanol and tin chloride in the silk solution are adjusted to promote the silk solution to form a silk film and solidify through β-ization, and cooperate with tin ions to firmly fix the silk molecules on the surface of the pre-finished fiber, thereby improving the antistatic performance of the prepared polyester fiber.

[0089] It can be seen from Examples 8-12 and Table 1 that, by placing the pre-finished fiber in a lipase treatment solution for immersion before the pre-finished fiber is immersed in the silk solution, the concentration of lipase in the prepared lipase treatment solution and the pH value of the lipase treatment solution are adjusted, so that the lipase hydrolyzes the ester bonds on the surface of the pre-finished fiber to generate polar carboxyl groups and carboxyl groups, which are convenient for subsequent combination with silk molecules and convenient for silk molecule monomers to penetrate into the polyester fiber, thereby improving the firmness of the silk molecules on the surface of the polyester fiber, and thus improving the antistatic properties of the prepared polyester fiber;

[0090] At the same time, the preparation method of the modified carbon black added in the preparation process of the polyester fiber is adjusted, and the mass ratio of the conductive carbon black to the chitosan in the preparation process is adjusted, so that the chitosan has a good wrapping effect on the conductive carbon black, and at the same time, it is also avoided that the wrapping layer formed by the chitosan on the conductive carbon black is too thick, which affects the conductive carbon black The effect of reducing the surface charge of the polyester fiber, the prepared modified carbon black has a good antistatic effect on the polyester fiber, and does not affect the breaking strength of the prepared antistatic polyester fiber.

[0091] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An antistatic polyester fiber, characterized in that: The invention is mainly made of the following raw materials in parts by weight: 40-50 parts of PET masterbatch, 20-30 parts of PET bottle flakes, and 3-5 parts of antistatic agent; the antistatic agent is composed of modified carbon black and nano-montmorillonite in a mass ratio of (2-4): (1-3); the preparation method of the modified carbon black comprises the following steps: 1) mixing conductive carbon black and titanate coupling agent to prepare an intermediate material; 2) The intermediate material obtained in step 1) is uniformly dispersed in the chitosan solution, dried and crushed to obtain a conductive carbon black having a mass ratio of (2-3) to chitosan: (3-5); The preparation method of the antistatic polyester fiber mainly comprises the following steps: S1: Mixing PET masterbatch, PET bottle flakes and antistatic agent together to prepare a mixed material; S2: placing the mixed material obtained in step S1 into a melt spinning machine for spinning to prepare pre-finished fiber, and then curling, oiling and cooling the pre-finished fiber; In step S2, before curling and oiling the pre-finished fiber, the pre-finished fiber is first immersed in a silk solution, wherein the silk solution comprises silk fibroin and hexafluoroisopropanol, and the mass ratio of the silk fibroin to the hexafluoroisopropanol is (7-10):(95-105).

2. The antistatic polyester fiber according to claim 1, characterized in that: Before use, the nano-montmorillonite in the antistatic agent is first immersed in a treatment liquid, and then taken out and dried; the treatment liquid includes a silane coupling agent.

3. The antistatic polyester fiber according to claim 1, characterized in that: The PET masterbatch is prepared by co-polymerization of sorbitol, ethylene glycol, terephthalic acid, isophthalic acid sulfonate and polyethylene glycol.

4. The antistatic polyester fiber according to claim 1, characterized in that: Ethanol and tin chloride are also added to the silk fibroin solution, and the mass ratio of the ethanol, tin chloride and silk fibroin is (3-5):(2-3):(8-10).

5. The antistatic polyester fiber according to claim 1, characterized in that: Before being immersed in the silk fibroin solution, the pre-finished fiber is first immersed in a lipase treatment solution, taken out for washing, and dried.

6. The antistatic polyester fiber according to claim 5, characterized in that: The concentration of lipase in the lipase treatment solution is 0.3-0.8 g / L.

7. The antistatic polyester fiber according to claim 5, characterized in that: The pH value of the lipase treatment solution is 6-10.