Preparation technology of impact-resistant photovoltaic tempered glass, double-glass components
Through the process of low-temperature glaze screen printing and corona treatment, the problem of high fragmentation rate of grid glass caused by the inconsistent expansion coefficient of the glaze layer and the glass is solved, and the impact resistance performance is improved and the service life of the components is extended.
Patent Information
- Application Number
- CN202310552018.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-05-16
AI Technical Summary
The existing grid glass has a high fragmentation rate during the curing process due to inconsistent expansion coefficients between the glaze layer and the glass. The problem becomes more serious especially as the size of the cells increases.
Use low-temperature glaze screen printing and bake at 110-240°C for 1-5 minutes to solidify, followed by corona treatment to prepare impact-resistant photovoltaic tempered glass to avoid stress concentration during the high-temperature tempering molding process.
The coating formed through the low-temperature curing process is flexible, significantly improves the impact resistance of tempered glass, reduces the fragmentation rate, extends the service life of the component, and reduces customer complaints and claims from the glass factory.
Smart Images

Figure CN116535103B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photovoltaic tempered glass, and in particular relates to a preparation process of impact-resistant photovoltaic tempered glass and a double-glass component. Background Art
[0002] The coating used for the mainstream grid glass on the market is glaze coating. The main components of the coating are low-melting-point glass powder, pigments, dispersants, solvents and a small amount of resin. The coating curing process is 100-150℃*1-2min solvent volatilization and 600-700℃*2-3min glass powder melting into glaze. The pigments and fillers will be wrapped by the glass glaze, and other organic components will be thermally decomposed and evaporated. The curing process of this coating is also the process of tempering the glass at the same time, which requires rapid heating and cooling. Because the expansion coefficients of the cured glaze layer and the tempered glass are inconsistent, after the glass cools down, a large concentrated stress will be generated between the glaze layer and the glass. In addition, the glass needs to be stacked and placed for transportation, so this kind of grid glass has a high fragmentation rate. Nowadays, the size of the battery cell is getting bigger and bigger, and the size of the glass has also increased by 20-40% on the original basis, which leads to a higher fragmentation rate of the glass after printing the glaze coating. The existing fragmentation rate of grid glass is 0.3-0.8%, and glass manufacturers are miserable.
[0003] Therefore, there is an urgent need for a grid tempered glass with low fragmentation rate and high impact resistance. Summary of the invention
[0004] The present invention provides a preparation process of impact-resistant photovoltaic tempered glass and a double-glass component, so as to solve the problem that the tempered glass prepared by the existing process is not impact-resistant and is easy to break.
[0005] In order to solve the above technical problems, the present invention provides a preparation process of impact-resistant photovoltaic tempered glass, comprising the following steps: step S1, preparing tempered glass; step S2, screen-printing a low-temperature glaze grid on the tempered glass; step S3, baking in a baking oven at 110-240°C for 1-5 minutes, and waiting for the low-temperature glaze to be fully cured and cross-linked to obtain a pre-prepared tempered glass; step S4, corona treating the pre-prepared tempered glass to obtain an impact-resistant photovoltaic tempered glass.
[0006] In yet another aspect, the present invention further provides a double-glass component, comprising impact-resistant photovoltaic tempered glass prepared by the preparation process as described above.
[0007] The beneficial effect of the present invention is that the preparation process of the impact-resistant photovoltaic tempered glass and the double-glass component of the present invention adopt low-temperature baking of low-temperature glaze to make the formed coating itself flexible. At the same time, because the process does not involve the high-temperature tempering and molding process of the glass, a large concentrated stress will not be formed on the glass surface, which effectively improves the impact resistance of the tempered glass. Therefore, no fragments will appear during the stacking, transportation or component use of the finished glass.
[0008] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practicing the present invention.
[0009] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0011] Figure 1 This is a process diagram for preparing the impact-resistant photovoltaic tempered glass of the present invention. DETAILED DESCRIPTION
[0012] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0013] The main reason for glass fragments is that low-melting-point glass powder is melted into glaze at 600-700℃, and 600-700℃ is also the process of glass tempering. The expansion coefficient of glass and the expansion coefficient of low-melting-point glass glaze are inconsistent, resulting in a large concentrated stress between the glass and the glass glaze. Therefore, glass fragments will appear during the stacking, transportation or use of finished glass components.
[0014] like Figure 1As shown, the present invention provides a preparation process of impact-resistant photovoltaic tempered glass, comprising the following steps: step S1, preparing tempered glass; step S2, screen-printing a low-temperature glaze grid on the tempered glass; step S3, baking in a baking oven at 110-240° C. for 1-5 min, waiting for the low-temperature glaze to be fully cured and cross-linked to obtain a pre-prepared tempered glass; step S4, corona treating the pre-prepared tempered glass to obtain an impact-resistant photovoltaic tempered glass.
[0015] In this embodiment, specifically, the components of the low-temperature glaze include the following raw materials in parts by mass: fluororesin: 60-100 parts; pigments and fillers: 50-75 parts; dispersant: 1-4 parts; modified polymer: 5-26 parts; leveling agent: 0.5-1.0 parts; antioxidant: 0.2-0.6 parts; blocked cyanate curing agent: 6-18 parts; catalyst: 0.1-0.4 parts; solvent: 35-60 parts; wherein the modified polymer is based on terminal hydroxyl polybutadiene, glycerol and maleic anhydride as the main chain, and both ends of the molecular chain are capped with N, N-(aminopropyltriethoxy) silane.
[0016] In this embodiment, specifically, the modified polymer includes the following components in parts by mass: terminal hydroxyl polybutadiene: 20.0-180.0 parts; glycerol: 0.5-3.0 parts; maleic anhydride: 4.0-8.0 parts; N,N-(aminopropyltriethoxy)silane: 7.0-9.0 parts; propylene glycol methyl ether acetate: 21.0-50.0 parts; the molecular weight Mn of the terminal hydroxyl polybutadiene is 1000-4500; the maleic anhydride needs to be dissolved in propylene glycol methyl ether acetate and then added dropwise.
[0017] In this embodiment, specifically, the fluororesin is one or more of tetrafluoroethylene-vinyl ether resin, tetrafluoroethylene-vinyl ester resin, trifluorochloroethylene-vinyl ether, trifluorochloroethylene-vinyl ester resin in FEVE resin; the hydroxyl value of the fluororesin is 50-80 mgKOH / g; specifically, such as Dongfu Chemical ZHM-2 or HLR-6 fluororesin, Changxing 41011 fluororesin, Daikin GK-570 fluororesin, etc.; the addition of fluororesin is to improve the weather resistance and dirt resistance of the coating, and it is one of the main film-forming materials of the coating.
[0018] In this embodiment, specifically, the low-temperature cured polyurethane coating itself is flexible and does not involve the high-temperature tempering process of the glass. It will not form a large stress concentration on the glass surface, so there will be no problem of fragmentation.
[0019] In this embodiment, specifically, the blocked polyisocyanate curing agent is one or more of a blocked HDI trimer, a blocked H6XDI adduct, and a blocked XDI adduct; specifically, Covestro's 3175 blocked isocyanate curing agent; each molecule of the blocked polyisocyanate curing agent carries two or more blocked -NCO groups, and the blocked curing agent is inactive at room temperature. The blocked curing agent is unblocked and released at high temperature, so that the -NCO group is released, and the -NCO group can react with the -OH in the coating component to form a network cross-linked structure, so that the physical and chemical properties of the coating can be stably maintained for a long time.
[0020] In this embodiment, specifically, the pigments and fillers are one or more of titanium dioxide, precipitated barium sulfate, lead sulfate, zinc oxide, calcium carbonate, copper chrome black, iron chrome black, carbon black, aniline black, iron red, cadmium red, lithol red, scarlet, cadmium yellow, lead chrome yellow, ultramarine, phthalocyanine blue, peacock blue, chrome green, zinc green, cobalt violet, ultramarine violet, silica, kaolin, bentonite, glass powder, hollow glass microbeads, alumina powder, PTFE micropowder, PVDF micropowder, PE wax powder, and PP wax powder; the addition of pigments and fillers is mainly to give color and enhance hiding power; it also has a certain influence on the rheology, weather resistance, chemical resistance, heat resistance, mechanical properties and feel of the coating, and the addition of pigments and fillers can also reduce the cost of the coating; some pigments and fillers also affect the flame retardancy and conductivity of the coating.
[0021] In this embodiment, specifically, the dispersant is one or more of anionic wetting dispersants, cationic wetting dispersants, nonionic wetting dispersants, amphoteric wetting dispersants, polymeric hyperdispersants, and controlled free radical hyperdispersants; specifically, Efka PU 4010; a dispersant is a surfactant having two opposite properties of lipophilicity and hydrophilicity in the molecule, which can reduce the time and energy required to complete the dispersion process, modify the surface properties of the particles, and adjust the mobility of the pigment particles, thereby improving the stability of the powder and avoiding flocculation and sedimentation.
[0022] In this embodiment, specifically, the leveling agent is one or more of an acrylic leveling agent, a silicone leveling agent, a fluorosilicone leveling agent and a high-boiling point solvent; the boiling point of the high-boiling point solvent is above 150°C; specifically, BYK-300; the leveling agent migrates to the wet film surface through limited compatibility, affects the surface tension of the paint film, and prompts the paint to form a smooth and uniform coating during the drying process, improves the permeability of the paint to the substrate, and reduces spots, marks and other appearance defects produced during painting.
[0023] In this embodiment, specifically, the antioxidant is one or more of hindered amines, hindered phenols, phosphites, thiodipropionates, and thiols; specifically, antioxidants such as 1010, 1076, 164, and 168; antioxidants are a type of substance that delays or inhibits thermal oxidative decomposition of polymers, which can delay aging of polymers and extend their service life.
[0024] In this embodiment, specifically, the catalyst is one or more of organic tin, organic zinc, organic bismuth, and amine; specifically, dibutyltin dilaurate; the catalyst is added to lower the deblocking temperature of the closed catalyst, and the active groups such as -OH, -COOH, amino, epoxy, etc. in the catalytic coating accelerate the reaction with the -NCO group, thereby improving production efficiency and avoiding incomplete reaction of the components in the coating, resulting in sticky coating and poor performance.
[0025] In this embodiment, specifically, the solvent is one or more of 783 slow-drying water, diethylene glycol butyl ether, dibasic acid ester, butyl acetate, toluene, xylene, ethyl acetate, propylene glycol methyl ether acetate, n-butanol, acetone, butanone, and No. 200 solvent oil; the solvent can dissolve the organic reactants to form a homogeneous system, so that the components in the coating are fully and evenly reacted and cross-linked. Solvents with different boiling points are selected according to the baking temperature to ensure that the coating is not sticky and has sufficient cross-linking and curing time. The use of some high-boiling point solvents can also meet the slow-drying and low-odor requirements of screen printing.
[0026] In this embodiment, specifically, low-melting-point glass powder is used in the glaze coating on the traditional grid glass. In order to lower the melting point, the low-melting-point glass powder needs to add sodium-potassium alkali metal components when the glass is mixed at high temperature. This sodium-potassium alkali metal component will be released when the crystalline silicon module is packaged and used for a long time, resulting in PID failure, that is, potential induced decay, which affects the service life of the photovoltaic module. In addition, the peeling strength of the traditional glaze coating with the adhesive film is significantly attenuated after PCT short-term wet heat aging and double 85 long-term wet heat aging, and water vapor easily penetrates into the module, resulting in leakage failure of the module; while the thermosetting coating used in the present invention has no alkali metal components, has excellent anti-PID effect, and the peeling strength of the coating and the adhesive film is less attenuated after wet heat aging.
[0027] In this embodiment, specifically, the mesh size of the screen printing is 80 to 200 meshes.
[0028] In this embodiment, specifically, the thickness of the screen-printed low-temperature glaze grid is 5-25 μm.
[0029] In this embodiment, specifically, the corona intensity of the corona treatment is 3-5 kW.
[0030] Embodiment 1:
[0031] The coating was prepared, stirred and screen-printed according to the formula ratio shown in Table 1. The oven baking temperature was 110-220°C, the baking time was 2 minutes, and the corona intensity was 4.5kW.
[0032] Table 1
[0033]
[0034]
[0035] Embodiment 2:
[0036] The coating was prepared, stirred and screen-printed according to the formula ratio shown in Table 2. The oven baking temperature was 110-240°C, the baking time was 2 minutes, and the corona intensity was 4.5kW.
[0037] Table 2
[0038] type Specific composition / ratio Dosage / weight Fluorine resin HLR-6 fluororesin 86 Pigments and Fillers Titanium dioxide: precipitated barium sulfate: bentonite = 6:2:1 72 Dispersants BYK-111 2.9 Modified polymer Modified polymer 12 Leveling agent BYK-306 0.8 Antioxidants 1076 0.5 Closed curing agent Mitsui G282 sealed curing agent 11 catalyst Organotin Catalyst 0.2 Solvents Butyl acetate 38
[0039] Embodiment 3:
[0040] The coating was prepared, stirred and screen-printed according to the formula ratio shown in Table 3. The oven baking temperature was 110-220°C, the baking time was 2 minutes, and the corona intensity was 4.5kW.
[0041] Table 3
[0042]
[0043]
[0044] Embodiment 4:
[0045] The coating was prepared, stirred and screen-printed according to the formula ratio shown in Table 4. The oven baking temperature was 110-230°C, the baking time was 2 minutes, and the corona intensity was 4.5kW.
[0046] Table 4
[0047] type Specific composition / ratio Dosage / weight Fluorine resin HLR-6 fluororesin 86 Pigments and Fillers Copper chrome black:silicon dioxide=15:1 52 Dispersants EFKA 4310 2.5 Modified polymer Modified polymer 25 Leveling agent BYK-331 0.5 Antioxidants 1076:168=6:1 0.5 Closed curing agent Covestro 3175 sealed curing agent 9 catalyst Organotin Catalyst 0.2 Solvents Xylene:Butyl acetate=1:1 42
[0048] Embodiment 5:
[0049] The coating was prepared, stirred and screen-printed according to the formula ratio shown in Table 5. The oven baking temperature was 110-230°C, the baking time was 2 minutes, and the corona intensity was 4.5kW.
[0050] Table 5
[0051]
[0052] Example test results:
[0053] Table 6 Initial performance
[0054]
[0055] Table 7 Aging performance
[0056]
[0057] Appendix: PID test refers to IEC TS 62804-2:2022; drop ball test refers to GB / T 15763.2-2005 impact resistance test.
[0058] From the above test results, we can see that:
[0059] (1) All of the examples in groups 1, 2, 3, 4, and 5 are low-temperature thermosetting grid glass coatings. Compared with the glazed grid glass coatings, the initial performance of the five groups of thermosetting coatings is basically the same as that of the glazed coatings, with no significant difference.
[0060] (2) In terms of PCT and double 85 wet heat aging, the peel strength of the glazed coating decays significantly, which is not as good as the low-temperature thermosetting coating;
[0061] (3) In the PID test, the glaze layer in the enameled grid glass has the risk of electrical breakdown, which will cause the cell to fail, while the low-temperature thermosetting coating has no abnormalities;
[0062] (4) In the ball drop test, the glazed grid glass has a certain probability of breaking, while the low-temperature thermosetting coated grid glass will not break.
[0063] It can be seen that although the present invention needs to add coating baking and corona treatment steps, it also reduces the glass fragmentation rate and reduces customer complaints and claims received by glass factories, which is a positive benefit in the long run; and as photovoltaic modules become larger and larger, the larger the glass, the greater the probability of fragmentation. Under the trend of larger glass sizes, the impact-resistant photovoltaic tempered glass prepared by the present invention has higher benefits.
[0064] At the same time, the components produced by the impact-resistant photovoltaic tempered glass of the present invention have no PID failure risk, and the coating performance does not significantly decay under long-term wet and hot aging conditions, which can effectively extend the service life of the components.
[0065] In yet another aspect, the present invention further provides a double-glass component, comprising impact-resistant photovoltaic tempered glass prepared by the preparation process as described above.
[0066] In summary, the preparation process of the impact-resistant photovoltaic tempered glass and the double-glass component of the present invention adopt low-temperature baking of low-temperature glaze to make the formed coating itself flexible. At the same time, because the process does not involve the high-temperature tempering and molding process of the glass, a large concentrated stress will not be formed on the glass surface, which effectively improves the impact resistance of the tempered glass. Therefore, no fragments will appear during the stacking, transportation or use of the finished glass.
[0067] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A process for preparing impact-resistant photovoltaic tempered glass, characterized in that: The steps include: Step S1, preparing tempered glass; Step S2, screen printing a low-temperature glaze grid on the tempered glass; Step S3, baking in a baking oven at 110-240° C. for 1-5 minutes, until the low-temperature glaze is fully cured and cross-linked to obtain the pre-prepared tempered glass; Step S4, corona treating the pre-prepared tempered glass to obtain impact-resistant photovoltaic tempered glass; The components of the low-temperature glaze include the following raw materials in parts by mass: Fluororesin: 60-100 parts; Pigments and fillers: 50-75 parts; Dispersant: 1-4 parts; Modified polymer: 5-26 parts; Leveling agent: 0.5-1.0 part; Antioxidant: 0.2-0.6 parts; Blocked cyanate curing agent: 6-18 parts; Catalyst: 0.1-0.4 parts; Solvent: 35-60 parts; The modified polymer is based on terminal hydroxyl polybutadiene, glycerol and maleic anhydride as main chains, and both ends of the molecular chain are capped with N, N-(aminopropyltriethoxy) silane.
2. The preparation process according to claim 1, characterized in that: The modified polymer comprises the following components in parts by weight: Hydroxyl-terminated polybutadiene: 20.0-180.0 parts; Glycerin: 0.5-3.0 parts; Maleic anhydride: 4.0-8.0 parts; N,N-(aminopropyltriethoxy)silane: 7.0-9.0 parts; Propylene glycol methyl ether acetate: 21.0-50.0 parts; The molecular weight Mn of the hydroxy-terminated polybutadiene is 1000 to 4500; The maleic anhydride needs to be dissolved in propylene glycol methyl ether acetate and then added dropwise.
3. The preparation process according to claim 1, characterized in that: The fluororesin is one or more of tetrafluoroethylene-vinyl ether resin, tetrafluoroethylene-vinyl ester resin, chlorotrifluoroethylene-vinyl ether resin and chlorotrifluoroethylene-vinyl ester resin in FEVE resin; The fluororesin has a hydroxyl value of 50-80 mgKOH / g.
4. The preparation process according to claim 1, characterized in that: The blocked polyisocyanate curing agent is one or more of a blocked HDI trimer, a blocked H6XDI adduct, and a blocked XDI adduct.
5. The preparation process according to claim 1, characterized in that: The pigment filler is one or more of titanium dioxide, precipitated barium sulfate, lithopone, zinc oxide, calcium carbonate, copper chrome black, iron chrome black, carbon black, aniline black, iron red, cadmium red, lithol red, scarlet, cadmium yellow, lead chrome yellow, ultramarine, phthalocyanine blue, peacock blue, chrome green, zinc green, cobalt violet, ultramarine violet, silicon dioxide, kaolin, bentonite, glass powder, hollow glass microspheres, alumina powder, PTFE micropowder, PVDF micropowder, PE wax powder, and PP wax powder; The dispersant is one or more of anionic wetting dispersants, cationic wetting dispersants, nonionic wetting dispersants, amphoteric wetting dispersants, polymeric super dispersants, and controlled free radical super dispersants; The leveling agent is one or more of an acrylic leveling agent, an organic silicon leveling agent, a fluorosilicone leveling agent and a high boiling point solvent; The antioxidant is one or more of hindered amines, hindered phenols, phosphites, thiodipropionates, and thiols; The catalyst is one or more of organotin, organozinc, organobismuth and amine; The solvent is one or more of 783 slow-drying water, diethylene glycol butyl ether, dibasic acid ester, butyl acetate, toluene, xylene, ethyl acetate, propylene glycol methyl ether acetate, n-butanol, acetone, butanone, and No. 200 solvent oil.
6. The preparation process according to claim 1, characterized in that: The mesh number of the screen printing is 80 to 200 meshes.
7. The preparation process according to claim 1, characterized in that: The thickness of the screen-printed low-temperature glaze mesh is 5 to 25 μm.
8. The preparation process according to claim 1, characterized in that: The corona intensity of the corona treatment is 3-5 kW.
9. A double-glass component, characterized in that: It comprises impact-resistant photovoltaic tempered glass prepared by the preparation process according to any one of claims 1 to 8.
Citation Information
Patent Citations
Manufacturing technology of colorful crystal toughened glass decoration panel having stereoscopic water drop effect
CN105015245A
Rubber composition for environment-friendly engineering tire, and preparation method thereof
CN111073077A
Processing method of high-strength backboard glass for solar double-glass assembly
CN114975659A
Coating film and coated article based thereon
CN115491067A
Photovoltaic backboard and photovoltaic module
CN115714147A