A method for preparing hyperbranched modified enzymatic lignin epoxy resin and its application
By preparing hyperbranched modified enzymatic lignin epoxy resin containing phosphorus, nitrogen and silicon, and combining diglycidyl ether to form an interlaced mesh structure, the problem of insufficient flame retardant performance of carbon fiber prepreg is solved, and safety is improved. The efficient utilization of enzymatic lignin waste is achieved.
Patent Information
- Application Number
- CN202310543824.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-15
AI Technical Summary
The flame retardant performance of existing carbon fiber prepregs is poor, making it difficult to achieve flame retardant, low smoke and low toxicity when exposed to open flames, affecting passenger safety, and enzymatic lignin waste has not been efficiently utilized.
The hyperbranching modifier containing phosphorus, nitrogen and silicon is prepared by raw materials such as phosphorus, silanol compounds, aliphatic diols, triethanolamine, etc., and the hyperbranching modification with epoxy groups is prepared by reacting with enzymatic lignin. Enzymatic lignin epoxy resin is used to improve the flame retardant properties of the prepreg, and react with diglycidyl ether compounds to form an interlaced network structure.
It significantly improves the flame retardant performance of carbon fiber prepreg, enhances its safety in high-temperature environments, and avoids damage to mechanical properties, achieving efficient reuse of enzymatic lignin waste.
Smart Images

Figure BDA0004229036570000062 
Figure BDA0004229036570000063
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon fiber prepregs, and particularly relates to a preparation method of a hyperbranched modified enzymatically hydrolyzed lignin epoxy resin and application thereof. Background Art
[0002] Carbon fiber prepreg, as the intermediate material of carbon fiber composite materials, is a product made by impregnating reinforced carbon fiber in matrix resin to form prepreg sheets. The matrix resin accounts for 30-40wt%, and the matrix resin used mainly includes polyester resin, epoxy resin, etc. Compared with other materials, the prepreg products can improve strength, fatigue strength, hardness, wear resistance, impact resistance, corrosion resistance, lightweight and other characteristics. They are mostly used in aviation, transportation, civil engineering and other fields. Among them, the seat products in transportation vehicles are the most common specific applications of carbon fiber prepreg in our daily life.
[0003] Seats are important safety components in transportation vehicles such as cars, high-speed trains, and airplanes. When using carbon fiber prepreg to make seat frames, its safety performance must be tested and measured from the aspects of static strength, stiffness, dynamic impact, and fatigue strength. For example, the inventor disclosed in the previous patent application CN202010867778.8 a hyperbranched polyether-modified lignin epoxy resin and its carbon fiber composite prepreg, the prepreg includes the following raw materials in parts by weight: 20-30 parts of bisphenol A epoxy resin, 9-14 parts of hyperbranched polyether-modified lignin epoxy resin, 50-80 parts of carbon fiber, 1-2 parts of latent curing agent, and 0.4-0.7 parts of accelerator. Patent CN202010618114.8 discloses a star-shaped polyester modified lignin epoxy resin and its carbon fiber composite prepreg, the prepreg comprising the following raw materials: 20-30 parts of bisphenol A epoxy resin, 12-18 parts of star-shaped polyester modified lignin epoxy resin as described in any one of claims 1-5, 40-70 parts of carbon fiber, 1-2 parts of latent curing agent, 0.4-0.7 parts of accelerator. Enzymatic lignin is lignin extracted from the residue of microbial enzymatic hydrolysis of corn stalks to prepare energy alcohol. Enzymatic lignin is generally used as solid waste landfill or direct combustion together with the residue, with low economic benefits, and biomass resources are not efficiently utilized. The above patented technology involves the reuse of enzymatic lignin, all of which are based on the characteristics of a large number of rigid aromatic rings, active phenolic hydroxyl groups, and alcoholic hydroxyl groups on enzymatic lignin to prepare enzymatic lignin-based epoxy resin-type "toughening agents", which improve the safety performance of carbon fiber prepregs from the perspective of improving the toughness and fatigue resistance of carbon fiber prepregs.
[0004] But it is well known that in addition to the mechanical properties of carbon fiber prepreg having an important impact on seat safety, seats are also affected by the particularity of the application space environment. Whether the seat manufacturing materials are flame retardant and the quality of flame retardant properties are also important criteria for testing and judging safety. If carbon fiber prepreg can be flame retardant, low smoke and low toxic after encountering open flames, it will greatly improve the personal safety of passengers.
[0005] The epoxy resin in the carbon fiber prepreg of the above patented technology is a flammable resin. Although the enzymatic lignin-based epoxy resin is a good carbon-forming agent, the flame retardant performance of the prepreg is poor if it is not used in conjunction with an acid source or a gas source. Therefore, the development of a flame-retardant bio-based carbon fiber prepreg is not only of great significance for improving the safety of seats, but also has significant economic value and far-reaching social significance for the research on the recycling of enzymatic lignin waste. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for preparing a hyperbranched modified enzymatic lignin epoxy resin and its application. Firstly, phosphoric acid, silanol compounds, aliphatic diols and triethanolamine are used as raw materials to prepare a hyperbranched modifier containing phosphorus, nitrogen and silicon, then the enzymatic lignin is modified by the hyperbranched modifier, and finally a diglycidyl ether compound is used to react with the modified product to prepare a hyperbranched modified enzymatic lignin epoxy resin with epoxy groups. The phosphorus, nitrogen and silicon in the epoxy resin are combined with the enzymatic lignin containing a large number of benzene rings to improve the flame retardant properties of the prepreg. In addition, the surface of the hyperbranched modified enzymatic lignin epoxy resin contains active epoxy groups, so that it can react with a curing agent and form a mutually interlaced network structure with the epoxy resin, which will not cause damage to the mechanical properties of the material compared with physically adding flame retardants.
[0007] In order to achieve the above objectives, the following specific technical solutions are adopted:
[0008] In a first aspect, the present invention provides a method for preparing a hyperbranched modified enzymatically hydrolyzed lignin epoxy resin, comprising the following steps:
[0009] 1) adding a water-carrying agent to a reaction kettle, heating the kettle to a reflux state, dropping a phosphoric acid aqueous solution, maintaining the reflux state for dehydration after the dropping, then adding a silanol compound, reacting under the reflux state, cooling to room temperature after the reaction, drying, extracting, and obtaining a monosubstituted phosphate compound for standby use;
[0010] 2) adding the monosubstituted phosphate compound, aliphatic diol and water-carrying agent obtained in step 1) into a reaction kettle, stirring evenly, heating and keeping the temperature constant for reaction, continuing to heat and keep the temperature constant for reaction, cooling to room temperature after the reaction is completed, and distilling under reduced pressure to obtain a phosphate oligomer;
[0011] 3) adding the phosphate oligomer obtained in step 2), triethanolamine, amino protective agent and water-carrying agent to an organic solvent, stirring evenly, heating and keeping the temperature constant for reaction, continuing to heat and keeping the temperature constant for reaction, cooling to room temperature after the reaction is completed, adjusting the pH, adding water until no precipitate is generated, filtering, washing the precipitate with water, acid washing, washing with water again, and drying to obtain a hyperbranched modifier;
[0012] 4) adding the hyperbranched modifier, enzymatic lignin, amino protective agent and water-carrying agent obtained in step 3) into a reaction kettle, stirring evenly, heating up and keeping the temperature constant for reaction, continuing to heat up and keep the temperature constant for reaction until the enzymatic lignin is completely dissolved, cooling down and keeping the temperature constant, adding diglycidyl ether compound, stirring until uniform reaction, adjusting pH after the reaction, washing with water, acid washing, washing with water again, and vacuum drying to obtain hyperbranched modified enzymatic lignin epoxy resin.
[0013] The molar ratio of the phosphoric acid, the silanol compound, the aliphatic diol and the triethanolamine is 1:1-1.05:0.89-0.95:0.15-0.25.
[0014] The weight ratio of the hyperbranched modifier, enzymatic lignin and diglycidyl ether compound is 3-5:1:7-10.
[0015] The concentration of the phosphoric acid aqueous solution is 80-90 wt %.
[0016] The silanol compound is selected from one or a combination of two or more of 3-(trimethylsilyl)-1-propanol, 3-triethylsilylpropan-1-ol, 2-(triethylsilyl)ethanol, 1-trimethylsilyl-2-propanol, 2-trimethylsilylpropan-1-ol, 2-(trimethylsilyl)ethanol, and hydroxybutyltrimethylsilane.
[0017] The aliphatic diol is a C2-C5 aliphatic straight-chain diol, selected from one or a combination of two or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,5-pentanediol.
[0018] The amino protective agent is selected from p-toluenesulfonic acid, benzenesulfonic acid or a combination of the two. The amino protective agent is used to prevent phosphoric acid and triethanolamine from generating tertiary amine phosphoric acid salt in the presence of water.
[0019] The water-carrying agent is selected from one or a combination of two or more of petroleum ether, benzene, toluene, xylene, cyclohexane, chloroform, carbon tetrachloride, and acetone.
[0020] The epoxy equivalent of the diglycidyl ether compound is 150-300 g / mol, and the diol diglycidyl ether is selected from one or a combination of polyethylene glycol diglycidyl ether and polypropylene glycol diglycidyl ether.
[0021] The enzymatically hydrolyzed lignin is obtained by an organic solvent extraction method, wherein the extraction solvent is selected from dioxane, ethanol, and methanol organic solvents. The weight average molecular weight of the enzymatically hydrolyzed lignin is 1000-3000, and the alcohol hydroxyl content is 3.3-3.8 wt %.
[0022] In order to improve the esterification rate of phosphoric acid and silanol compounds in step 1) and the esterification rate of phosphoric acid esterification reaction involved in steps 2) to 4), an azeotropic dehydration method is used for the reaction.
[0023] Step 1) The amount of the water-carrying agent is 1-1.2 times the total weight of the phosphoric acid aqueous solution and the silanol compound, the phosphoric acid aqueous solution is dripped in 1-3 hours, and the dehydration time is 1-3 hours; the reaction time under the reflux state is to stop the reaction when the molar amount of distilled water is 0.95-1.0 times the molar amount of phosphoric acid, the drying is carried out with an inorganic desiccant, the inorganic desiccant is not limited to anhydrous magnesium sulfate, and the solvent used for the extraction is one or a combination of two of ether and chloroform;
[0024] Step 2) The amount of the water-carrying agent is 30-40wt% of the total weight of phosphoric acid, silanol compounds, and aliphatic diols; the temperature is raised to 120°C-150°C, and the reaction time is 3-5h; the continued temperature increase is raised to 150°C-180°C, and the reaction time is 1-3h;
[0025] Step 3) The amount of the amino protective agent is 1-1.3 times the molar number of triethanolamine; the amount of the water-carrying agent is 25-30wt% of the weight of phosphoric acid, silanol compounds, aliphatic diols, and triethanolamine; the temperature is raised to 120°C-150°C, and the reaction time is 3-5h; the continued temperature is raised to 180°C-200°C, and the reaction time is 1-3h; the pH is adjusted to neutral with a saturated sodium bicarbonate solution, the acid washing is washed 1-5 times with a 30-37wt% hydrochloric acid solution, and the number of times of the second water washing is 1-5 times;
[0026] The amount of the water-carrying agent in step 4) is 20-25wt% of the total weight of phosphoric acid, silanol compounds, aliphatic diols, triethanolamine, and enzymatically hydrolyzed lignin; the amount of the amino protective agent is 1-1.3 times the molar number of triethanolamine in step 3); the heating is raised to 120°C-150°C, and the reaction time is 3-5h; the continued heating is raised to 180-200°C, and the reaction time is 1-3h; the cooling is lowered to 30-50°C, and the reaction time is 3-5h; the pH is adjusted to neutral with a saturated sodium bicarbonate solution, the water washing is to remove sodium p-toluenesulfonic acid salt, the acid washing is to wash 1-5 times with a 30-37wt% hydrochloric acid solution of the same volume as the reaction mixture, and the second water washing is to wash away the residual hydrochloric acid on the reaction mixture.
[0027] In a second aspect, the present invention provides a hyperbranched modified enzymatically hydrolyzed lignin epoxy resin, wherein the hyperbranched modified enzymatically hydrolyzed lignin epoxy resin is obtained by the preparation method described in the first aspect.
[0028] In a third aspect, the present invention provides a carbon fiber prepreg composite material, which comprises the following raw materials in parts by weight: 20-30 parts of epoxy resin, 10-15 parts of the above-mentioned hyperbranched modified enzymatic lignin epoxy resin, 50-80 parts of carbon fiber, 1-2 parts of curing agent, and 0.5-1 part of curing accelerator.
[0029] The epoxy value of the epoxy resin is 0.20-0.44.
[0030] The carbon fiber is not particularly limited, and any commonly used carbon fiber in the art may be used.
[0031] The curing agent is selected from one or a combination of two or more of dicyandiamide, methyltetrahydrophthalic anhydride, benzoyl hydrazide, and adipic acid dihydrazide.
[0032] The curing accelerator is an imidazole curing accelerator, which can be selected from one or a combination of two or more of imidazole cyanurate, 2-methylimidazole cyanurate, 2-ethyl cyanurate, and 2-phenylimidazole cyanurate.
[0033] The carbon fiber prepreg composite material can be used as a raw material for seats in transportation vehicles.
[0034] The preparation method of the hyperbranched modified enzymatically hydrolyzed lignin epoxy resin comprises the following steps:
[0035] S1: adding epoxy resin and the above-mentioned hyperbranched modified enzymatic lignin epoxy resin into a mixing kettle, heating and stirring until the mixture is uniform, adding curing agent and curing accelerator, continuing to stir until uniform, discharging the material to a coating machine for coating, and obtaining a film;
[0036] S2: Compound the adhesive film prepared in step S1 with carbon fiber on a compounding machine, pull the carbon fiber out from the sand rack and arrange it neatly through the fiber yarn arrangement roller, and enter the compounding roller of the compounding machine synchronously with the adhesive film, heat and compound, and then cool and reel it up to obtain the carbon fiber prepreg.
[0037] The temperature in step S1 is raised to 90-130°C.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The invention firstly uses phosphoric acid, silanol compounds, aliphatic diols and triethanolamine as raw materials to prepare a hyperbranched modifier containing phosphorus, nitrogen and silicon, then uses the hyperbranched modifier to modify enzymatic lignin, and finally uses diglycidyl ether compounds to react with the modified product to prepare a hyperbranched modified enzymatic lignin epoxy resin with epoxy groups. The phosphorus, nitrogen and silicon in the epoxy resin are combined with the enzymatic lignin containing a large number of benzene rings to improve the flame retardant performance of the prepreg. In addition, the surface of the hyperbranched modified enzymatic lignin epoxy resin contains active epoxy groups, so that it can react with a curing agent and form a mutually interlaced network structure with the epoxy resin, and compared with physically adding a flame retardant, no mechanical property damage of the material is caused. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.
[0041] Enzymatic lignin was purchased from Shanxi Biomass New Materials Industry Research Institute Co., Ltd., with a weight average molecular weight of 1000-3000 and an alcohol hydroxyl content of 3.5wt%;
[0042] Polyethylene glycol diglycidyl ether was purchased from Wuhan Haishan Technology Co., Ltd., with an epoxy equivalent of 220 g / mol;
[0043] Carbon fiber was purchased from Toray, Japan, T300, 3K.
[0044] Preparation of hyperbranched modified enzymatic lignin epoxy resin
[0045] Preparation Example 1
[0046] 1) Add 400 mL of xylene to a reaction kettle, raise the temperature to reflux, dropwise add 116.1 g of 85 wt% phosphoric acid aqueous solution (1.0 mol of phosphoric acid), keep the reflux state for dehydration for 90 min after the dropwise addition for 2 h, then add 132.3 g of 3-(trimethylsilyl)-1-propanol (1.0 mol), react under reflux until the amount of distilled water is 18 g (1 mol), stop the reaction, cool to room temperature, dry with anhydrous magnesium sulfate, extract with chloroform, and obtain a monosubstituted phosphate compound for use.
[0047] 2) The monosubstituted phosphate compound obtained in step 1), 180.2 g of 1,4-butanediol (0.89 mol) and 94 g of xylene were added to a reactor, stirred evenly, heated to 130° C. and reacted at a constant temperature for 3 h, then heated to 150° C. and reacted at a constant temperature for 2 h. After the reaction was completed, the reaction was cooled to room temperature, and the water-carrying agent and unreacted 1,4-butanediol were removed by reduced pressure distillation to obtain a phosphate oligomer; acid value: 1.24 mmol / g.
[0048] 3) The phosphate oligomer obtained in step 2), 179.04 g triethanolamine (0.15 mol), 27.3 g p-toluenesulfonic acid (0.15 mol), and 100 g xylene are added to an organic solvent, stirred evenly, heated to 130° C. and reacted at a constant temperature for 5 h, then heated to 180° C. and reacted at a constant temperature for 3 h. After the reaction, the mixture was cooled to room temperature, adjusted to neutrality with saturated sodium bicarbonate solution, and a large amount of water was added until no precipitation was produced. The mixture was filtered, and the precipitate was washed 3 times with water, 3 times with 30 wt% hydrochloric acid solution, and then washed 3 times with water, and dried to obtain a hyperbranched modifier.
[0049] 4) 300 g of the hyperbranched modifier obtained in step 3), 100 g of enzymatic lignin, 206.64 g of p-toluenesulfonic acid, and 140 g of xylene were added to a reactor, stirred evenly, heated to 130° C. and reacted at a constant temperature for 5 h, and then heated to 180° C. and reacted at a constant temperature until the enzymatic lignin was completely dissolved, cooled to 50° C. and kept at a constant temperature, and 1000 g of polyethylene glycol diglycidyl ether was added, stirred until uniform and reacted for 5 h. After the reaction was completed, a saturated sodium bicarbonate solution was added to adjust to neutrality, the water was separated, and the mixture was washed 3 times with an equal volume of water to the obtained mixture, the water was separated, and the mixture was washed 3 times with an equal volume of 30 wt % hydrochloric acid solution to the obtained mixture, and then washed 3 times with an equal volume of water to the obtained mixture, the water was separated, and the mixture was dried in vacuo to obtain a hyperbranched modified enzymatic lignin epoxy resin with a viscosity of 6900 mPa·s.
[0050] The reaction of Example 1 and the product structure are shown below:
[0051] Step 1)
[0052] Step 2)
[0053] Step 3) Reaction of the branching unit of the hyperbranched modifier obtained:
[0054]
[0055] Linear Unit:
[0056] End Unit:
[0057] wherein a, b, m, n, x, y and z are independently selected from any integer of 1-20.
[0058] Preparation Example 2
[0059] The rest is the same as Preparation Example 1, except that 3-(trimethylsilyl)-1-propanol in step 1) is replaced by 3-triethylsilylpropane-1-propanol in an equal molar amount. The obtained hyperbranched modified enzymatically hydrolyzed lignin epoxy resin has a viscosity of 6900 mPa·s.
[0060] Preparation Example 3
[0061] The rest is the same as Preparation Example 1, except that the amount of polyethylene glycol diglycidyl ether is 700 g. The viscosity of the obtained hyperbranched modified enzymatically hydrolyzed lignin epoxy resin is 5600 mPa·s.
[0062] Preparation Example 4
[0063] The rest is the same as Preparation Example 1, except that 1000 g of an equal amount of butanediol diglycidyl ether is used to replace polyethylene glycol diglycidyl ether. The viscosity of the obtained hyperbranched modified enzymatically hydrolyzed lignin epoxy resin is 7700 mPa·s.
[0064] Comparative Preparation Example 1
[0065] The rest is the same as Preparation Example 1, except that 3-(trimethylsilyl)-1-propanol in step 1) is replaced by an equimolar amount of methanol. The obtained hyperbranched modified enzymatically hydrolyzed lignin epoxy resin has a viscosity of 7400 mPa·s.
[0066] Preparation of flame-retardant bio-based carbon fiber prepreg
[0067] Example 1
[0068] S1: 18 parts of E44, 12 parts of E20, and 15 parts of the hyperbranched modified enzymatic lignin epoxy resin prepared in Preparation Example 1 are added to a mixing kettle, heated to 110°C and stirred until uniformly mixed, 2 parts of dicyandiamide and 0.8 parts of imidazole cyanurate are added, stirring is continued until uniformly mixed, and the material is discharged to a coating machine for coating to obtain a film;
[0069] S2 composites the adhesive film prepared in step S1 with carbon fiber on a composite machine, pulls 70 parts of carbon fiber out from the sand rack and arranges them neatly through five groups of fiber yarn arrangement rollers (the weight is controlled by the fiber arrangement thickness and the width of the carbon fiber during the preparation process), and simultaneously enters the composite roller of the composite machine with 1 layer of adhesive film, undergoes two heating composites and then cools and reels, to obtain a unidirectional carbon fiber prepreg with a square gram weight of 175g.
[0070] Example 2
[0071] The rest is the same as Example 1, except that the hyperbranched modified enzymatic lignin epoxy resin is prepared according to Preparation Example 2.
[0072] Example 3
[0073] The rest is the same as Example 1, except that the hyperbranched modified enzymatic lignin epoxy resin is prepared according to Preparation Example 3.
[0074] Example 4
[0075] The rest is the same as Example 1, except that the hyperbranched modified enzymatic lignin epoxy resin is prepared according to Preparation Example 4.
[0076] Example 5
[0077] The rest is the same as Example 1, except that 12 parts of E44, 8 parts of E20, 10 parts of the hyperbranched modified enzymatic lignin epoxy resin prepared in Preparation Example 1, 1 part of dicyandiamide, and 0.5 parts of imidazole cyanurate are used.
[0078] Comparative Example 1
[0079] The rest is the same as Example 1, except that the hyperbranched modified enzymatic lignin epoxy resin is prepared according to Comparative Preparation Example 1.
[0080] Application Example 1
[0081] The flame-retardant bio-based carbon fiber prepreg prepared in Example 1 was cut, laid on a mold, assembled and placed in a mold, and pressurized and cured at a curing temperature of 120° C. for 2 hours to prepare a carbon fiber composite material sheet.
[0082] Application Examples 2-5, Comparative Application Example 1
[0083] The rest is the same as Application Example 1, except that the flame-retardant bio-based carbon fiber prepregs used correspond to those prepared in Examples 2-5 and Comparative Example 1, respectively.
[0084] Preparation Example Step 2) Method for determining the acid value of the product obtained:
[0085] Take 2-3g of the product obtained in step 2) and add it to a 150g conical flask, dissolve it with 30mL of 1:1 methanol solution, add 3-5 drops of phenolphthalein reagent, and then titrate with standard solution. When the solution turns slightly pink, it is the titration end point. Calculate the acid value according to the following formula.
[0086] Acid value = (C × V) / m, mmol
[0087] Wherein C = standard concentration of KOH, mol / L; V = standard KOH solution consumed in titration, mL; m = mass of the product of step 2), g.
[0088] The carbon fiber composite materials prepared in the above application examples 1-5 and comparative application example 1 were subjected to the following performance tests:
[0089] Shear strength: Refer to standard JC / T 773-2010 to test interlayer shear strength.
[0090] Flame retardant properties: tested in accordance with EN 45545-2.
[0091] Impact strength: Tested with reference to GB / T 1451-2005 fiber reinforced plastic simply supported beam impact toughness test method.
[0092] Table 1
[0093] project Shear strength MPa Flame retardant grade <![CDATA[Impact strength kJ / m 2 > Application Example 1 88.7 HL3 77.1 Application Example 2 88.5 HL3 77.0 Application Example 3 86.8 HL3 73.7 Application Example 4 80.4 HL3 77.8 Application Example 5 84.2 HL3 80.5 Comparative application example 1 75.1 HL2 76.7
[0094] It can be seen from Table 1 that the carbon fiber prepreg prepared by the present invention has good flame retardancy and mechanical strength. From the poor flame retardancy results of the carbon fiber composite material plate in Application Example 1 and Comparative Application Example 1, it can be seen that the addition of silicon helps to further improve the flame retardancy of the composite material by coordinating the intumescent flame retardant composed of the acid source, gas source and carbon source; and the use of 3-(trimethylsilyl)-1-propanol in combination with polyethylene glycol diglycidyl ether can improve the wettability of the base resin to the carbon fiber and improve the shear strength.
[0095] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.
Claims
1. A method for preparing a hyperbranched modified enzymatically hydrolyzed lignin epoxy resin, characterized in that: The following steps are involved: 1) adding a water-carrying agent to a reaction kettle, heating the kettle to a reflux state, dropping a phosphoric acid aqueous solution, maintaining the reflux state for dehydration after the dropping, then adding a silanol compound, reacting under the reflux state, cooling to room temperature after the reaction, drying, extracting, and obtaining a monosubstituted phosphate compound for standby use; 2) adding the monosubstituted phosphate compound, aliphatic diol and water-carrying agent obtained in step 1) into a reaction kettle, stirring evenly, heating and keeping the temperature constant for reaction, continuing to heat and keep the temperature constant for reaction, cooling to room temperature after the reaction is completed, and distilling under reduced pressure to obtain a phosphate oligomer; 3) adding the phosphate oligomer obtained in step 2), triethanolamine, amino protective agent and water-carrying agent to an organic solvent, stirring evenly, heating and keeping the temperature constant for reaction, continuing to heat and keeping the temperature constant for reaction, cooling to room temperature after the reaction is completed, adjusting the pH, adding water until no precipitate is generated, filtering, washing the precipitate with water, acid washing, washing with water again, and drying to obtain a hyperbranched modifier; 4) adding the hyperbranched modifier, enzymolysis lignin, amino protective agent and water-carrying agent obtained in step 3) into a reaction kettle, stirring evenly, heating and keeping the temperature constant for reaction, continuing to heat and keep the temperature constant for reaction until the enzymolysis lignin is completely dissolved, cooling and keeping the temperature constant, adding diglycidyl ether compounds, stirring until uniform reaction, adjusting pH after the reaction, washing with water, acid washing, washing with water again, and vacuum drying to obtain a hyperbranched modified enzymolysis lignin epoxy resin; the molar ratio of the phosphoric acid, the silanol compound, the aliphatic diol and the triethanolamine is 1:1-1.05:0.89-0.95:0.15-0.25; the weight ratio of the hyperbranched modifier, the enzymolysis lignin and the diglycidyl ether compounds is 3-5:1:7-10.
2. The method for preparing a hyperbranched modified enzymatic lignin epoxy resin according to claim 1, wherein: The silanol compound is selected from one or a combination of two or more of 3-(trimethylsilyl)-1-propanol, 3-triethylsilylpropan-1-ol, 2-(triethylsilyl)ethanol, 1-trimethylsilyl-2-propanol, 2-trimethylsilylpropan-1-ol, 2-(trimethylsilyl)ethanol, and hydroxybutyltrimethylsilane; the aliphatic diol is a C2-C5 aliphatic straight-chain diol, selected from one or a combination of two or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,5-pentanediol.
3. The method for preparing a hyperbranched modified enzymatic lignin epoxy resin according to claim 1, wherein: The epoxy equivalent of the diglycidyl ether compound is 150-300 g / mol, and the diol diglycidyl ether is selected from one or a combination of polyethylene glycol diglycidyl ether and polypropylene glycol diglycidyl ether; the enzymatically hydrolyzed lignin is obtained by organic solvent extraction, and the weight average molecular weight of the enzymatically hydrolyzed lignin is 1000-3000, and the alcohol hydroxyl content is 3.3-3.8wt%.
4. The method for preparing a hyperbranched modified enzymatic lignin epoxy resin according to claim 1, wherein: Step 2) The amount of the water-carrying agent is 30-40wt% of the total weight of phosphoric acid, silanol compounds, and aliphatic diols; the temperature is raised to 120°C-150°C, and the reaction time is 3-5h; the continued temperature increase is raised to 150°C-180°C, and the reaction time is 1-3h; Step 3) The amount of the amino protective agent is 1-1.3 times the molar number of triethanolamine; the amount of the water-carrying agent is 25-30wt% of the sum of the weight of phosphoric acid, silanol compounds, aliphatic diols, and triethanolamine; the temperature is raised to 120°C-150°C, and the reaction time is 3-5h; the continued temperature increase is raised to 180°C-200°C, and the reaction time is 1-3h; In step 4), the amount of the water-carrying agent is 20-25wt% of the total weight of phosphoric acid, silanol compounds, aliphatic diols, triethanolamine, and enzymatically hydrolyzed lignin; the amount of the amino protective agent is 1-1.3 times the molar number of triethanolamine in step 3); the temperature is raised to 120°C-150°C, and the reaction time is 3-5h; the continued temperature increase is raised to 180-200°C, and the reaction time is 1-3h; the temperature reduction is reduced to 30-50°C, and the reaction time is 3-5h.
5. A hyperbranched modified enzymatic lignin epoxy resin, characterized in that: The hyperbranched modified enzymatically hydrolyzed lignin epoxy resin is obtained by the preparation method according to any one of claims 1 to 4.
6. A carbon fiber prepreg composite material, comprising the following raw materials in parts by weight: 20-30 parts of epoxy resin, 10-15 parts of the hyperbranched modified enzymatic lignin epoxy resin according to any one of claims 1-4, 50-80 parts of carbon fiber, 1-2 parts of curing agent, and 0.5-1 part of curing accelerator.
7. The carbon fiber prepreg composite material according to claim 6, characterized in that: The epoxy value of the epoxy resin is 0.20-0.
44.
8. The method for preparing the carbon fiber prepreg composite material according to claim 6 or 7, characterized in that: The steps include: S1: adding epoxy resin and hyperbranched modified enzymatic lignin epoxy resin into a mixing kettle, heating and stirring until the mixture is uniform, adding curing agent and curing accelerator, continuing to stir until the mixture is uniform, discharging the material to a coating machine for coating, and obtaining a film; S2: Compound the adhesive film prepared in step S1 with carbon fiber on a compounding machine, pull the carbon fiber out from the sand rack and arrange it neatly through the fiber yarn arrangement roller, and enter the compounding roller of the compounding machine synchronously with the adhesive film, heat and compound, and then cool and reel it up to obtain the carbon fiber prepreg.
Citation Information
Patent Citations
Star-shaped polyester modified lignin epoxy resin and carbon fiber composite prepreg thereof
CN111607066A
Silicon-nitrogen-phosphate coordinating flame retardant epoxy resin powder coating suitable for steel tube and preparation method of silicon-nitrogen-phosphate coordinating flame retardant epoxy resin powder coating
CN104448237A
Hyperbranched silicon-phosphorus synergistic flame retardant modified epoxy resin and preparation method thereof
CN110591288A
High-toughness flame-retardant medium-and-low-temperature cured epoxy resin system and preparation method thereof
CN110628000A
Hyperbranched polyether modified lignin epoxy resin and carbon fiber composite prepreg thereof
CN111944121A