A detection and analysis method for feldspar dissolution rate under near-equilibrium-dynamic equilibrium conditions
By mixing feldspar mineral powder with water and immersing it in a saturated solution for reaction, combined with scanning electron microscopy and laser confocal scanning three-dimensional map analysis, the problem of inaccurate evaluation of feldspar dissolution rate in the prior art is solved, and the problem of being unable to accurately evaluate feldspar dissolution rate in realization The precise detection of feldspar dissolution rate under near-balanced-dynamic equilibrium state is of great research significance.
Patent Information
- Application Number
- CN202310541759.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-15
AI Technical Summary
The prior art is difficult to accurately evaluate the dissolution rate of feldspar minerals under high temperature semi-enclosed-closed conditions (near-equilibrium-dynamic equilibrium state). Traditional methods cannot effectively evaluate the dissolution rate through ion changes, resulting in the inability to correctly evaluate the dissolution condition.
Under a carbon dioxide atmosphere, feldspar mineral powder is mixed with water to form a saturated solution, and then the polished feldspar sheets are immersed in the solution for reaction. The morphological changes of feldspar surface are analyzed by scanning electron microscopy and laser confocal scanning three-dimensional diagram to calculate erosion Volume and rate to achieve accurate detection of feldspar dissolution rate in near-balanced-dynamic equilibrium state.
An indoor experimental method was established, which could quantitatively characterize feldspar dissolution rate under different temperature conditions, providing a research basis for the evolution and physical properties of closed environment reservoirs, and significantly improving the detection accuracy and intuitiveness of dissolution rate.
Smart Images

Figure CN116539845B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of feldspar dissolution, and in particular to a method for detecting and analyzing feldspar dissolution rate under near-equilibrium-dynamic equilibrium conditions. Background Art
[0002] Feldspar minerals are important skeleton particle components in clastic reservoirs in oil and gas basins around the world. There are many types of feldspar minerals and a wide distribution range, from the surface to the deep crust. The dissolution of feldspar plays an important and dominant role in the development of secondary pores and the improvement of physical properties in reservoirs. Therefore, the dissolution of feldspar has always been a hot topic in the field of water-rock interaction. At present, scholars at home and abroad focus on studying the dissolution mechanism, dissolution rate and controlling factors of feldspar in a relatively open environment of low temperature to high temperature. However, the research on the dissolution dynamics and quantitative prediction of feldspar minerals under high temperature semi-closed-closed conditions (water-rock system is in a near-equilibrium-dynamic equilibrium state) is relatively weak. In addition, the current evaluation of feldspar dissolution rate is often determined by testing the relationship between ion changes in the reaction solution and reaction time. However, when the water-rock system is in a near-equilibrium-dynamic equilibrium state, the ions in the reaction solution only change slightly or do not change. Therefore, ordinary methods can no longer make a correct evaluation of the dissolution rate of feldspar in a near-equilibrium-dynamic equilibrium state. Therefore, it is of great significance to establish a more accurate, more intuitive and more complete method to evaluate the dissolution rate of feldspar in a near-equilibrium-dynamic equilibrium state. Summary of the invention
[0003] The purpose of the present invention is to overcome the problems existing in the prior art and provide a method for detecting and analyzing the dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a method for detecting and analyzing the dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions, comprising the following steps:
[0006] (1) mixing feldspar mineral powder with water under a carbon dioxide atmosphere to react and obtain a saturated solution;
[0007] (2) In a carbon dioxide atmosphere, the feldspar slice is immersed in a saturated solution for reaction, and then the dissolution rate of the feldspar is detected.
[0008] Preferably, the particle size of the feldspar mineral powder in step (1) is 80 to 120 meshes.
[0009] Preferably, in step (1), the mass ratio of the feldspar mineral powder to water is 0.9-1.1:10-10.1.
[0010] Preferably, the reaction temperature in step (1) is 80-160°C.
[0011] Preferably, the reaction pressure in step (1) is 0.1-1.8 MPa.
[0012] Preferably, the reaction time of step (1) is 50 to 70 days.
[0013] Preferably, the reaction temperature in step (2) is 80-160°C.
[0014] Preferably, the reaction pressure in step (2) is 0.1-1.8 MPa.
[0015] Preferably, the reaction time in step (2) is 10 to 20 days.
[0016] The beneficial effects of the present invention are:
[0017] The present invention provides a method for detecting and analyzing the dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions, comprising the following steps: mixing feldspar mineral powder with water under a carbon dioxide atmosphere, reacting to obtain a saturated solution; immersing a polished feldspar sheet in the saturated solution under a carbon dioxide atmosphere to react, detecting and analyzing the surface morphology changes of the feldspar after the reaction, and calculating the dissolution volume and dissolution rate of the feldspar. The present invention innovatively establishes an experimental method for quantitatively characterizing the dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions under different indoor temperature conditions. By analyzing the surface morphology changes of the polished feldspar sheet and combining chemical methods, the feldspar dissolution rate of the water-rock system in a near-equilibrium-dynamic equilibrium state is more accurately calculated, which is of great significance for solving the research on reservoir evolution and physical property improvement problems in a closed environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a schematic diagram of placing the feldspar flakes in the reactor in Example 1;
[0019] Figure 2 This is a scanning electron microscope characterization image of the feldspar flake in Example 1;
[0020] Figure 3 This is a three-dimensional laser confocal scanning image of the feldspar flake in Example 1;
[0021] Figure 4 This is a scanning electron microscope characterization image of the feldspar flake in Example 2;
[0022] Figure 5 This is a three-dimensional laser confocal scanning image of the feldspar flake in Example 2;
[0023] Figure 6 This is a scanning electron microscope characterization image of the feldspar flake in Example 3;
[0024] Figure 7 This is a three-dimensional laser confocal scanning image of the feldspar flake in Example 3;
[0025] Figure 8 This is a scanning electron microscope characterization image of the feldspar flake in Example 4;
[0026] Fig. 9 This is a three-dimensional laser confocal scanning image of the feldspar flake in Example 4;
[0027] Fig.10 This is a scanning electron microscope characterization image of the feldspar flake in Example 5;
[0028] Fig.11 This is a three-dimensional laser confocal scanning image of the feldspar flake in Example 5;
[0029] Fig.12 This is a scanning electron microscope characterization image of the feldspar flake in Example 6;
[0030] Fig.13 This is a three-dimensional laser confocal scanning image of the feldspar flake in Example 6. DETAILED DESCRIPTION
[0031] The present invention provides a method for detecting and analyzing the dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions, comprising the following steps:
[0032] (1) mixing feldspar mineral powder with water under a carbon dioxide atmosphere to react and obtain a saturated solution;
[0033] (2) In a carbon dioxide atmosphere, the feldspar slice is immersed in a saturated solution for reaction, and then the dissolution rate of the feldspar is detected.
[0034] In the present invention, the feldspar mineral powder in step (1) is obtained by crushing a feldspar mineral, and the feldspar mineral is preferably albite or potassium feldspar.
[0035] In the present invention, the particle size of the feldspar mineral powder in step (1) is preferably 80-120 mesh, more preferably 90-110 mesh, and even more preferably 95-105 mesh.
[0036] In the present invention, the feldspar mineral powder in step (1) is preferably pre-treated before use, and the pre-treatment comprises the following steps: washing the feldspar mineral powder with water, repeating the process until impurities on the surface of the mineral powder are completely removed, and then drying.
[0037] In the present invention, the drying temperature is preferably 50 to 70°C, more preferably 55 to 65°C, and even more preferably 57 to 63°C.
[0038] In the present invention, after drying, part of the feldspar mineral powder is taken out for gold spraying and then observed under a scanning electron microscope. The purpose is to ensure that the powder sample has been cleaned, and this part of the sample is no longer used in subsequent experiments.
[0039] In the present invention, the mass ratio of the feldspar mineral powder to water in step (1) is preferably 0.9-1.1:10-10.1, more preferably 0.95-1.05:10.02-10.08, and more preferably 0.97-1.03:10.04-10.06.
[0040] In the present invention, the reactions in step (1) and step (2) are preferably carried out in a high-temperature and high-pressure reactor (with an outer wall diameter of 20 mm, a thickness of 5 mm, and a height of 120 mm); the high-temperature and high-pressure reactor is washed with water before use, and the washing is repeated until impurities such as organic matter in the reactor are completely removed, and then dried.
[0041] In the present invention, the drying temperature is preferably 70-90°C, more preferably 75-85°C, and more preferably 77-83°C; the drying time is preferably 2.5-3.5h, more preferably 2.7-3.3h, and more preferably 2.8-3.2h.
[0042] In the present invention, the reaction temperature in step (1) is preferably 80 to 160°C, more preferably 90 to 150°C, and even more preferably 100 to 140°C.
[0043] In the present invention, the pressure of the reaction in step (1) is preferably 0.1 to 1.8 MPa, more preferably 0.3 to 1.6 MPa, and even more preferably 0.5 to 1.4 MPa.
[0044] In the present invention, the reaction time of step (1) is preferably 50 to 70 days, more preferably 55 to 65 days, and more preferably 57 to 63 days.
[0045] In the present invention, after the reaction in step (1) is completed, the saturated solution is taken out using a syringe, placed in a graphite bottle, and then placed in a blast drying oven to avoid ion precipitation due to temperature reduction, so that the solution remains in a saturated state; the temperature of the blast drying oven is preferably 40 to 60°C, more preferably 45 to 55°C, and more preferably 47 to 53°C.
[0046] In the present invention, the feldspar flakes in step (2) are obtained by grinding a feldspar mineral, and the feldspar mineral is preferably sodium feldspar or potassium feldspar. The type of the feldspar mineral here must be consistent with the type of the feldspar mineral used in step (1); the size (length×width×height) of the feldspar flakes after grinding is preferably 3.5-4.5 cm×0.5-1.5 cm×0.1-0.3 cm, more preferably 3.6-4.4 cm×0.6-1.4 cm×0.12-0.28 cm, and more preferably 3.8-4.2 cm×0.8-1.2 cm×0.15-0.25 cm.
[0047] In the present invention, the feldspar flakes in step (2) are preferably subjected to double-sided polishing before use, and the purpose of polishing is to ensure that the surface of the feldspar flakes is flat and smooth.
[0048] In the present invention, the preparation work before starting the reaction in step (2) comprises the following steps: injecting a saturated solution into a high-temperature and high-pressure reactor (the high-temperature and high-pressure reactor is also subjected to the above-mentioned water washing and drying steps before use), calculating the height of the saturated solution in the reactor, using paper to wrap a feldspar sheet, the length of the paper being equal to the height of the saturated solution in the reactor, spraying gold on the portion of the feldspar sheet not wrapped with the paper, then removing the paper, immersing the end not sprayed with gold in the saturated solution, installing the reactor (ensuring good sealing), injecting carbon dioxide gas into the reactor, and repeating the filling and deflation until the original gas in the reactor is exhausted.
[0049] In the present invention, the amount of the saturated solution is preferably 2 to 4 mL, more preferably 2.5 to 3.5 mL, and even more preferably 2.7 to 3.3 mL.
[0050] In the present invention, the reaction temperature in step (2) is preferably 80-160°C, more preferably 90-150°C, and more preferably 100-140°C; the reaction temperature here must be consistent with the reaction temperature in step (1).
[0051] In the present invention, the pressure of the reaction in step (2) is preferably 0.1-1.8 MPa, more preferably 0.3-1.6 MPa, and more preferably 0.5-1.4 MPa; the pressure of the reaction here must be consistent with the pressure of the reaction in step (1).
[0052] In the present invention, the reaction time of step (2) is preferably 10 to 20 days, more preferably 12 to 18 days, and even more preferably 14 to 16 days.
[0053] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0054] Example 1
[0055] The potassium feldspar was crushed to obtain feldspar mineral powder with a particle size of 100 mesh, and the feldspar mineral powder was washed with water, and the process was repeated until the impurities on the surface of the mineral powder were completely removed, and then dried at 30°C; a high-temperature and high-pressure reactor with an outer wall diameter of 20 mm, a thickness of 5 mm, and a height of 120 mm was washed with water, and the process was repeated until the organic matter and other impurities in the reactor were completely removed, and then dried at 80°C for 3h; 1.0g of feldspar mineral powder was mixed with 10.0g of water under a carbon dioxide atmosphere, and reacted for 60 days at a temperature of 80°C and a pressure of 0.1MPa to obtain a saturated solution; after the reaction was completed, the saturated solution was taken out with a syringe, placed in a graphite bottle, and then placed in a blast drying oven for standby use (the temperature of the blast drying oven was set to 50°C);
[0056] The potassium feldspar was polished to obtain a feldspar sheet with a size of 4cm×1cm×0.2cm, and the feldspar sheet was double-sided polished until the surface of the feldspar sheet was flat and smooth; a high-temperature and high-pressure reactor with an outer wall diameter of 20mm, a thickness of 5mm, and a height of 120mm was washed with water, and the process was repeated until the organic matter and other impurities in the reactor were completely removed, and then dried at 80°C for 3h; 3mL of saturated solution was injected into the high-temperature and high-pressure reactor, and the height of the saturated solution in the reactor was calculated to be 2cm. The feldspar sheet was wrapped with paper, and the length of the paper was 2cm. The part of the feldspar sheet not wrapped with paper was sprayed with gold, and then the paper was removed, and the end not sprayed with gold was immersed in the saturated solution, the reactor was installed (to ensure good sealing), and carbon dioxide gas was injected into the reactor, and the gas was repeatedly filled and discharged until the original gas in the reactor was exhausted; under the carbon dioxide atmosphere, the temperature was set to 80°C and the pressure was set to 0.1MPa, and the reaction was carried out for 15 days, and then the dissolution rate of the feldspar was detected.
[0057] The schematic diagram of placing the feldspar flakes in the reactor in this embodiment is as follows: Figure 1 shown.
[0058] After the reaction is completed, the feldspar flakes are taken out and placed in a sample bag, and the gas in the sample bag is emptied. The surface morphology of the feldspar flake dissolution section and the surface morphology of the feldspar flake gold spraying section are compared by a high-resolution desktop scanning electron microscope in the shortest possible time. The proportion of dissolution pits and dissolution cracks on the surface of the feldspar dissolution section and their morphological characteristics are observed, and compared with the gold spraying section to obtain a scanning electron microscope characterization image of the feldspar flake in this embodiment, as shown in FIG. Figure 2 shown; from Figure 2 It can be seen that after the reaction, the potassium feldspar dissolution pits are mostly filled with spherical mineral particles.
[0059] After the scanning electron microscope observation, the feldspar flakes were ultrasonically cleaned with distilled water for 10 minutes to wash away the secondary minerals on the surface of the feldspar flakes. The surface morphology of the feldspar flakes was quantitatively described using a KC laser confocal microscope. The dissolved section and the gold-sprayed section of the feldspar flakes were randomly scanned (the surrounding environment was kept free of noise and vibration to prevent errors caused by instrument vibration). The scanning range (length × width) was 0.1 cm × 0.1 cm. A three-dimensional map of the surface morphology of the feldspar flakes was constructed using the scanned data, and a laser confocal scanning three-dimensional map of the feldspar flakes in this embodiment was obtained, as shown in FIG. Figure 3 shown; from Figure 3 The morphological changes on the surface of the feldspar flakes can be analyzed more intuitively. The average height difference of the dissolution section minus the average height difference of the gold-spraying section is the average dissolution height h of the dissolution surface when the dissolution section is in a saturated solution.
[0060] The information on the surface morphology of feldspar flakes obtained by scanning electron microscopy and KC laser confocal microscopy was comprehensively analyzed to obtain the average height of the dissolution pits on the dissolution surface of the feldspar flakes (h), and the volume of the dissolution pits and dissolution cracks in the dissolution section of the feldspar flakes (C) was calculated. 3 , albite takes 2.625g / cm 3 ), the mass of feldspar dissolution (m) is calculated, and the amount of substance dissolved in feldspar (n) is obtained through the molar mass information of feldspar (M). The area of feldspar dissolution (S) and the experimental reaction time (t) are used to obtain the dissolution rate (V) of feldspar under near-equilibrium-dynamic equilibrium conditions.
[0061] The calculation process is as follows:
[0062]
[0063]
[0064]
[0065] After calculation, the feldspar dissolution amount in this example is 1.138×10 -8 cm 3 , the feldspar dissolution rate is 8.040×10 -15 mol / cm 2 / sec.
[0066] Example 2
[0067] While keeping other conditions in Example 1 unchanged, potassium feldspar was completely replaced by sodium feldspar, and the mass of feldspar mineral powder was changed to 1.06 g. After the reaction was completed, the dissolution rate of feldspar was detected.
[0068] The feldspar in this embodiment is tested by the same testing method as in Example 1, and a scanning electron microscope characterization image of the feldspar flake in this embodiment is obtained, as shown in FIG. Figure 4 shown; from Figure 4 It can be seen from the figure that after the reaction, the sodium feldspar dissolution pits are mostly filled with spherical mineral particles. The laser confocal scanning 3D image of the feldspar flake in this embodiment is as follows: Figure 5 As shown; after calculation, the feldspar dissolution amount in this embodiment is 1.772×10 -8 cm 3 , the feldspar dissolution rate is 1.365×10 -14 mol / cm 2 / sec.
[0069] Example 3
[0070] The other conditions in Example 1 were controlled to remain unchanged, the mass of distilled water was changed to 10.04 g, the reaction temperature was changed to 120° C., the reaction pressure was modified to 0.42 MPa, and the dissolution rate of feldspar was detected after the reaction was completed.
[0071] The feldspar in this embodiment is tested by the same testing method as in Example 1, and a scanning electron microscope characterization image of the feldspar flake in this embodiment is obtained, as shown in FIG. Figure 6 shown; from Figure 6 It can be seen from the figure that after the reaction, potassium feldspar dissolves and the spherical mineral particles decrease. The laser confocal scanning 3D image of the feldspar flake in this embodiment is as follows: Figure 7 As shown; after calculation, the feldspar dissolution amount in this embodiment is 2.094×10 -8 cm 3 , the feldspar dissolution rate is 1.479×10 -14 mol / cm 2 / sec.
[0072] Example 4
[0073] The other conditions in Example 1 were controlled to remain unchanged, potassium feldspar was completely replaced by sodium feldspar, the mass of feldspar mineral powder was changed to 0.99 g, the reaction temperature was changed to 120° C., the reaction pressure was modified to 0.42 MPa, and the dissolution rate of feldspar was detected after the reaction was completed.
[0074] The feldspar in this embodiment is tested by the same testing method as in Example 1, and a scanning electron microscope characterization image of the feldspar flake in this embodiment is obtained, as shown in FIG. Figure 8 shown; from Figure 8 It can be seen from the figure that after the reaction, the sodium feldspar dissolution pit is still filled with spherical mineral particles. The laser confocal scanning 3D image of the feldspar slice in this embodiment is as follows: Fig. 9 As shown; after calculation, the feldspar dissolution amount in this embodiment is 2.818×10-8 cm 3 , the feldspar dissolution rate is 2.169×10 -14 mol / cm 2 / sec.
[0075] Example 5
[0076] The other conditions in Example 1 were kept unchanged, the mass of the feldspar mineral powder was changed to 1.02 g, the reaction temperature was changed to 160° C., the reaction pressure was modified to 1.79 MPa, and the dissolution rate of the feldspar was detected after the reaction was completed.
[0077] The feldspar in this embodiment is tested by the same testing method as in Example 1, and a scanning electron microscope characterization image of the feldspar flake in this embodiment is obtained, as shown in FIG. Fig.10 shown; from Fig.10 It can be seen from the figure that after the reaction, potassium feldspar dissolves, spherical mineral particles disappear, and tiny flake minerals are attached to the surface of the feldspar flakes. The laser confocal scanning 3D image of the feldspar flakes in this embodiment is as follows: Fig.11 As shown; after calculation, the feldspar dissolution amount in this embodiment is 3.532×10 -8 cm 3 , the feldspar dissolution rate is 2.496×10 -14 mol / cm 2 / sec.
[0078] Example 6
[0079] The other conditions in Example 1 are controlled to remain unchanged, potassium feldspar is completely replaced by sodium feldspar, the mass of feldspar mineral powder is changed to 1.01 g, the mass of distilled water is changed to 10.05 g, the reaction temperature is changed to 160° C., the reaction pressure is modified to 1.79 MPa, and the dissolution rate of feldspar is detected after the reaction is completed.
[0080] The feldspar in this embodiment is tested by the same testing method as in Example 1, and a scanning electron microscope characterization image of the feldspar flake in this embodiment is obtained, as shown in FIG. Fig.12 shown; from Fig.12 It can be seen from the figure that after the reaction, the sodium feldspar dissolves and forms many dissolution cracks. The laser confocal scanning 3D image of the feldspar slice in this embodiment is as follows: Fig.13 As shown; after calculation, the feldspar dissolution amount in this embodiment is 3.991×10 -8 cm 3 , the feldspar dissolution rate is 3.074×10 -14 mol / cm 2 / sec.
[0081] It can be seen from the above embodiments that the present invention provides a method for detecting and analyzing the dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions. Under different near-equilibrium-dynamic equilibrium conditions of 80°C, 120°C, and 160°C, potassium feldspar and sodium feldspar minerals continue to dissolve, and after the experiment, secondary minerals can be seen covering the surface of the feldspar locally. The dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions is much lower than the dissolution rate under far-equilibrium conditions at the same temperature; the dissolution rates of potassium feldspar and sodium feldspar under different temperatures and far-equilibrium conditions are shown in Table 1.
[0082] Table 1 Dissolution rates of potassium feldspar and sodium feldspar at different temperatures and far-equilibrium conditions
[0083]
[0084] The present invention innovatively establishes an experimental method for quantitatively characterizing the feldspar dissolution rate in a near-equilibrium-dynamic equilibrium state under different indoor temperature conditions. By analyzing the surface morphology changes of polished feldspar flakes and combining chemical methods, the feldspar dissolution rate of the water-rock system in a near-equilibrium-dynamic equilibrium state is more accurately calculated, which is of great significance for solving the research problems of reservoir evolution and physical property improvement in a closed environment.
[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for detecting and analyzing the dissolution rate of feldspar under near-equilibrium-dynamic equilibrium conditions, characterized in that: It includes the following steps: (1) In a carbon dioxide atmosphere, feldspar mineral powder is mixed with water to react to obtain a saturated solution; (2) In a carbon dioxide atmosphere, the polished feldspar flakes are immersed in a saturated solution for reaction. At this time, the reaction is in a near-equilibrium-dynamic equilibrium state, and the ions in the reaction solution undergo only slight changes or no changes. (3) After the reaction, the information on the surface morphology of the feldspar flakes obtained by scanning electron microscopy and KC laser confocal microscopy was comprehensively analyzed to obtain the average height of the dissolution pits on the dissolution surface of the feldspar flakes. The volumes of the dissolution pits and dissolution cracks in the dissolution section of the feldspar flakes were calculated. Combined with the density of the feldspar flakes, the mass of the feldspar dissolution was calculated. The amount of the substance dissolved in the feldspar was obtained through the molar mass information of the feldspar. The area of the dissolved feldspar and the experimental reaction time were used to obtain the dissolution rate of the feldspar under near-equilibrium-dynamic equilibrium conditions.
2. The detection and analysis method according to claim 1, characterized in that: The particle size of the feldspar mineral powder in step (1) is 80-120 mesh.
3. The detection and analysis method according to claim 1 or 2, characterized in that: The mass ratio of the feldspar mineral powder to water in step (1) is 0.9-1.1:10-10.
1.
4. The detection and analysis method according to claim 3, characterized in that: The reaction temperature in step (1) is 80-160°C.
5. The detection and analysis method according to claim 4, characterized in that: The reaction pressure in step (1) is 0.1-1.8 MPa.
6. The detection and analysis method according to claim 4 or 5, characterized in that: The reaction time of step (1) is 50 to 70 days.
7. The detection and analysis method according to claim 6, characterized in that: The reaction temperature in step (2) is 80-160°C.
8. The detection and analysis method according to claim 7, characterized in that: The reaction pressure in step (2) is 0.1-1.8 MPa.
9. The detection and analysis method according to claim 7 or 8, characterized in that: The reaction time of step (2) is 10 to 20 days.