A polyamide composition and its preparation method and application
By rationally combining bis(hexamethylene)triamine and phthalic acid in halogen-free flame-retardant high-temperature nylon materials to form a cross-linked structure, combined with halogen-free flame retardants and reinforcing fillers, the problem of the material's viscosity decreasing at high temperatures is solved. problem, achieving the maintenance of viscosity and mechanical properties, and improving processing stability and performance.
Patent Information
- Application Number
- CN202310478625.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Halogen-free flame-retardant high-temperature nylon materials are prone to viscosity decline and decomposition at high temperatures, resulting in processing difficulties and product performance degradation. Existing technologies use antioxidants to improve stability, but the effect is not good and cannot effectively maintain viscosity and mechanical properties.
By rationally matching the dosage of bis(hexamethylene)triamine and phthalic acid to promote the formation of cross-linked structure and increase the viscosity, and combining it with halogen-free flame retardants and reinforcing fillers, a polyamide composition is prepared for Improve viscosity retention before and after processing and mechanical properties after heat retention.
It significantly improves the relative viscosity retention rate before and after processing and the capillary viscosity retention rate after heat retention, avoids the material's viscosity drop and loss of mechanical properties, and ensures the material's stability and processing performance.
Smart Images

Figure BDA0004206319610000021 
Figure BDA0004206319610000051 
Figure BDA0004206319610000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of modified polyamide, and specifically to a polyamide composition and a preparation method and application thereof. Background Art
[0002] At present, the new energy vehicle and consumer electronics industries are further developing in a highly integrated manner, and the volume requirements for parts are getting smaller and smaller. Therefore, SMT welding has gradually replaced traditional manual welding and wave soldering and become the mainstream of welding. However, the peak temperature of SMT can reach 260-270℃, which puts extremely high requirements on the temperature resistance of the product. Traditional PA66 and PBT materials cannot meet such harsh conditions at all. Therefore, a large number of products have begun to use halogen-free flame-retardant high-temperature nylon materials.
[0003] Halogen-free flame-retardant high-temperature nylon has benzene rings in its molecular weight, so its processing temperature is relatively high, which can reach 330-350℃. However, the amide bond in nylon is the most active group, and the amide bond will decompose to a certain extent when the temperature reaches 350℃. Even if the temperature does not reach the above temperature, there will be a certain trend of viscosity decrease, and the decrease in viscosity means that the material will have chain breaks and other behaviors. In production, there will be phenomena such as drooling during injection molding, strong odor, and unpleasant gas generation. In the use of materials, there will be problems such as decreased strength and increased gas marks on the surface of the parts. Therefore, some foreign customers have put forward clear requirements for the viscosity retention rate before and after nylon processing.
[0004] At present, there is little research in the industry on the viscosity maintenance of halogen-free flame-retardant high-temperature nylon before and after processing. Some patents refer to the experience of PA66 and other materials and increase the stability of the material by using more antioxidants. However, since the antioxidant itself is also a small molecule and the processing temperature of high-temperature nylon materials is extremely high, the antioxidant will decompose, which will cause a decrease in the strength of the system. The solutions provided by the current existing technologies are only temporary solutions and do not address the root cause. Summary of the invention
[0005] In order to overcome the above-mentioned defects of the prior art, the present invention proposes a polyamide composition and a preparation method and application thereof. The specific technical scheme is as follows:
[0006] A polyamide composition, comprising the following components in parts by weight:
[0007]
[0008] The added bis(hexamethylene)triamine will promote the cross-linking of the system at high temperature, thereby increasing the viscosity. At the same time, terephthalic acid will promote the extension of the molecular chain, which will also increase the viscosity. However, the cross-linking structure will lead to a sharp increase in the viscosity of the system, but the actual reaction amount is not high. The cross-linking structure will greatly increase the viscosity, but the number of end groups that actually react is insufficient, resulting in poor mechanics. The single diamine will not lead to an obvious increase in viscosity. Although it reacts, it is still a linear structure and cannot maintain the viscosity.
[0009] The present application can achieve a balance between the increase in viscosity and the decomposition of the material at high temperature by reasonably matching the dosage of bis(hexamethylene)triamine and terephthalic acid, thereby achieving the purpose of maintaining viscosity. That is, by using bis(hexamethylene)triamine and terephthalic acid in combination, compared with antioxidants, significantly improved relative viscosity before and after processing and better retention rate of capillary viscosity before and after thermal retention can be obtained, as well as improved mechanical properties after retention.
[0010] Furthermore, the purity of the bis(hexamethylene)triamine is greater than or equal to 98 wt %.
[0011] Furthermore, the purity of the terephthalic acid is greater than or equal to 99wt%.
[0012] Furthermore, the weight ratio of the bis(hexamethylene)triamine to terephthalic acid is 1:(1-3).
[0013] Preferably, the weight ratio of the bis(hexamethylene)triamine to terephthalic acid is 1:2.
[0014] Furthermore, the halogen-free flame retardant is diethyl aluminum hypophosphite.
[0015] Furthermore, the reinforcing filler is selected from one or more of fibrous reinforcing materials or flat reinforcing materials.
[0016] Furthermore, the fibrous reinforcing material is selected from one or more of glass fiber and carbon fiber, and the flat plate reinforcing material is selected from one or more of talc and mica.
[0017] The present invention also provides a method for preparing the polyamide composition, comprising the following steps:
[0018] S1: weighing each component according to the ratio, and premixing each component except the halogen-free flame retardant and the reinforcing filler to obtain a premix;
[0019] S2: feeding the premix of step S1 into an extruder, adding a reinforcing filler into a first side feed port of the extruder, adding a halogen-free flame retardant into a second side feed port of the extruder, performing melt blending and extrusion granulation to obtain the polyamide composition.
[0020] Furthermore, the extruder is a twin-screw extruder, and the processing temperature of the melt blending is 290-330°C.
[0021] The present invention also provides applications of the polyamide composition in consumer electronics and new energy vehicles, such as new energy high-voltage connectors, automotive board-to-line connectors, DDR5 memory cards, and the like.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The application, through the use amount of bis(hexamethylene)triamine and terephthalic acid, has overcome the cross-linked structure of bis(hexamethylene)triamine and greatly increased viscosity, but the actual reaction of the end group number is insufficient, making the defect of poor mechanics. It has also overcome the fact that a single diamine can bring about an unobvious increase in viscosity, although it reacts, it is still a linear structure and cannot bring about the defect of maintaining viscosity. It can be achieved that the relative viscosity before and after processing and the capillary viscosity before and after heat retention are better maintained, and the viscosity of the material after processing will not be caused to drop significantly or rise, thereby causing the situation of various bad processing problems, and the mechanical retention rate before and after heat retention can be effectively improved. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] <Preparation of Examples and Comparative Examples>
[0026] The raw materials used in the examples and comparative examples of the present invention are commercially available or homemade, but are not limited to these materials:
[0027] Semi-aromatic polyamide A: homemade, according to the ratio, add decanediamine, terephthalic acid, benzoic acid end-capping agent and deionized water into a reactor with nitrogen atmosphere and pressure of 2.8Mpa, heat the reactor to 180°C, keep the temperature constant for 0.5-1.5 hours, then heat to 235°C, keep the temperature constant for 10-15 hours to obtain PA10T;
[0028] Semi-aromatic polyamide B: homemade, according to the ratio, hexamethylenediamine, terephthalic acid, benzoic acid end-capping agent and deionized water were added into a reactor with nitrogen atmosphere and pressure of 2.8Mpa, the reactor was heated to 180°C, kept at this temperature for 0.5-1.5 hours, then heated to 235°C, kept at this temperature for 10-15 hours to obtain PA6T;
[0029] Halogen-free flame retardant: diethyl aluminum hypophosphite, purchased from Clariant;
[0030] Bis(hexamethylene)triamine: purity 98wt%, purchased from Anergy;
[0031] Terephthalic acid: purity 99wt%, purchased from Anaiji;
[0032] Glass fiber: brand ECS301 HP, purchased from Chongqing International Composite Materials Co., Ltd.;
[0033] Molecular sieve: 5A molecular sieve, purchased from Guangdong Xintao Technology;
[0034] Antioxidant: NAUGARD 445, Clariant.
[0035] The preparation methods of the embodiments of the present invention and the comparative examples are as follows:
[0036] S1: According to the ratios in Table 1 and Table 3, weigh each component, and premix each component except the halogen-free flame retardant and the reinforcing filler to obtain a premix;
[0037] S2: The premix of step S1 is fed into a twin-screw extruder, a reinforcing filler is added into a first side feed port of the twin-screw extruder, and a halogen-free flame retardant is added into a second side feed port of the twin-screw extruder, melt blending is performed at a processing temperature of 300° C., and extrusion granulation is performed to obtain a polyamide composition.
[0038] The twin-screw extruder had a screw length-to-diameter ratio of 52:1, a barrel temperature of 300°C, a screw speed of 200 rpm, and a feed rate of 350 Kg / h.
[0039] <Test Standard>
[0040] The performance test standards of the embodiments and comparative examples of the present invention are as follows:
[0041] Tensile strength test before and after retention: According to ISO 527-1 / -2:2012 injection molding standard tensile test strip 115*10*4mm, and strength test is carried out at 10mm / min, which is the tensile strength before retention; according to ISO 527-1 / -2:2012 injection molding standard tensile test strip, but during injection molding, the material residence time on the machine is extended to 20min, and then strength test is carried out according to the standard, which is the tensile strength after retention;
[0042] Relative viscosity test before and after processing: Polyamide relative viscosity test method: refer to GB12006.1-89, polyamide viscosity number determination method; the specific test method is: measure the relative viscosity ηr of polyamide with a concentration of 0.25g / dl in 98% concentrated sulfuric acid at 25±0.01℃; test the particles before injection molding as the viscosity before processing; cut the material from the injection molding national standard sample for viscosity test as the viscosity after processing;
[0043] Capillary viscosity test before and after retention: The test was carried out under a capillary rheometer at 330°C and a shear rate of 1000s -1 The cavity is filled with plastic particles under the conditions of , firstly, it is plasticized for 5 min, and then the viscosity is measured and used as the initial capillary viscosity, and then it is retained for 15 min and the viscosity is measured and used as the capillary viscosity after retention.
[0044] Table 1. Formula of Examples 1-8 (parts by weight)
[0045]
[0046]
[0047] Table 2. Performance test results of Examples 1-8
[0048]
[0049] Table 3. Comparative Examples 1-9 formulations (parts by weight)
[0050]
[0051]
[0052] Table 4. Performance test results of comparative examples 1-9
[0053]
[0054] Compared with Example 3, in Comparative Examples 1 and 2, too much or too little (hexamethylene) triamine usage will result in a decrease in the material's tensile strength retention rate, the relative viscosity retention rate before and after processing, and the capillary viscosity retention rate before and after retention. The weight ratio of the bis(hexamethylene) triamine to terephthalic acid is 1:(1-3). Preferably, the weight ratio of the bis(hexamethylene) triamine to terephthalic acid is 1:2.
[0055] Compared with Example 3, the amount of terephthalic acid added in Comparative Example 3 is too much, and the tensile strength retention rate of Comparative Example 3 is increased, but the viscosity increases sharply, causing the material to lose fluidity and be completely unable to be processed; compared with Example 3, the amount of terephthalic acid added in Comparative Example 4 is too little, and the tensile strength retention rate, relative viscosity retention rate before and after processing, and capillary viscosity retention rate before and after retention of Comparative Example 4 are reduced.
[0056] Compared with Example 3, Comparative Examples 5, 6, and 7 do not add bis(hexamethylene)triamine, terephthalic acid, and do not add bis(hexamethylene)triamine and terephthalic acid, respectively. The tensile strength retention rate, relative viscosity retention rate before and after processing, and capillary viscosity retention rate before and after retention of Comparative Examples 5-7 are all inferior to those of Comparative Example 3.
[0057] Compared with Example 3, in Comparative Example 8, the use of molecular sieves or antioxidants is not effective in improving the tensile strength retention rate, the relative viscosity retention rate before and after processing, and the capillary viscosity retention rate before and after retention.
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyamide composition, characterized in that By weight, it includes the following components:
2. The polyamide composition according to claim 1, characterized in that The semi-aromatic polyamide includes one or more of PA10T and PA6T.
3. The polyamide composition according to claim 1, characterized in that The weight ratio of the bis(hexamethylene)triamine to terephthalic acid is 1:(1-3).
4. The polyamide composition according to claim 3, characterized in that The weight ratio of the bis(hexamethylene)triamine to terephthalic acid is 1:
2.
5. The polyamide composition according to claim 1, characterized in that The halogen-free flame retardant is diethyl aluminum hypophosphite.
6. The polyamide composition according to claim 1, characterized in that The reinforcing filler is selected from one or more of fibrous reinforcing materials or flat plate reinforcing materials.
7. The polyamide composition according to claim 6, characterized in that The fibrous reinforcement material is selected from one or more of glass fiber and carbon fiber.
8. The polyamide composition according to claim 6, characterized in that The flat plate reinforcing material is selected from one or more of talc and mica.
9. A method for preparing a polyamide composition according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: Weigh each component according to the ratio, and premix each component except the halogen-free flame retardant and the reinforcing filler to obtain a premix; S2: feeding the premix of step S1 into an extruder, adding a reinforcing filler into a first side feed port of the extruder, adding a halogen-free flame retardant into a second side feed port of the extruder, performing melt blending and extrusion granulation to obtain the polyamide composition.
10. Use of the polyamide composition according to any one of claims 1 to 8 in consumer electronics and new energy vehicles.
Citation Information
Patent Citations
High-gloss enhanced polyamide compound and preparation method thereof
CN102863790A
Polyamide composite material with high weld mark strength as well as preparation method and application thereof
CN114656785A