A carbon molecular sieve membrane and its preparation method and application
Through rare earth salt coordination modification and control of carbonization conditions, the pore structure of the carbon molecular sieve membrane is improved, which solves the problems of complex preparation process and insufficient gas separation performance in the existing technology, and realizes a carbon molecular sieve membrane with high gas permeability and selectivity. , suitable for a variety of gas purification applications.
Patent Information
- Application Number
- CN202310684572.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-09
AI Technical Summary
In the existing technology, the preparation process of carbon molecular sieve membranes is complex, the carbonization temperature is high or the thermal reshaping temperature is difficult to control, which limits its industrial application, and the gas separation performance is insufficient.
By adding rare earth salts for rare earth coordination modification, and controlling the temperature and atmosphere during the carbonization process, the pore structure and gas separation performance of the carbon molecular sieve membrane are improved. Polymers such as polyamide, polybenzimidazole, etc. are used as precursors. Rare earth salts such as gadolinium chloride, ytterbium chloride, etc. form carbon molecular sieve membranes with high gas permeability and selectivity.
The preparation process is simplified, the gas separation performance of the carbon molecular sieve membrane is improved, high gas permeability and selectivity are achieved, and it is suitable for gas purification of natural gas, water gas and synthesis gas.
Smart Images

Figure CN116571099B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of separation membranes, and in particular relates to a carbon molecular sieve membrane and a preparation method and application thereof. Background Art
[0002] Carbon molecular sieve membranes have high thermal stability, high chemical stability and excellent gas separation performance. Carbon molecular sieve membranes are usually carbonized from polymers as precursors. During the carbonization process, the polymer molecular chains are gradually transformed into layered carbon structures with graphitization characteristics. The defects formed by the accumulation of interlayers constitute the microporous structure and ultramicroporous structure in the carbon molecular sieve membrane. Among them, the larger micropores provide high specific surface area and high gas permeability, while the ultramicropores control the diffusion selectivity of the membrane. Unlike the pore structure of conventional molecular sieves (such as MOF, zeolite, etc.), the pore size of carbon molecular sieve membranes is uneven and distributed in an amorphous state, showing a unique pore structure distribution and excellent gas separation performance. The pore structure and gas separation performance of carbon molecular sieve membranes are greatly affected by precursors and carbonization conditions.
[0003] CN107635646A discloses a super-selective carbon molecular sieve membrane and a manufacturing method. The manufacturing method obtains a highly selective carbon molecular sieve membrane by increasing the carbonization temperature of a polyimide hollow fiber membrane. The membrane can be used for the separation of CO2 / CH4, O2 / N2 and N2 / CH4. However, the carbonization temperature of this technical solution is too high, which not only increases the difficulty of processing, but also makes the carbon molecular sieve membrane more brittle, limiting further industrial applications.
[0004] CN112044273A discloses a method for preparing a carbon molecular sieve membrane with improved permeability and selectivity and its application, wherein the preparation method improves the free volume and pore structure distribution of the precursor by thermally reshaping the polymer precursor near the glass transition temperature, thereby improving the gas permeability of the carbon molecular sieve membrane after carbonization. However, the technical solution has high requirements for the control of the thermal reshaping temperature, which increases the difficulty of industrial production.
[0005] CN105621389A discloses a method for preparing a supported composite carbon molecular sieve membrane, wherein the preparation method introduces MOF into a polymer precursor and then performs high-temperature carbonization to obtain a carbon molecular sieve membrane with excellent gas separation performance. However, the complicated preparation steps of this technical solution bring a certain degree of difficulty to the processing of the carbon molecular sieve membrane.
[0006] Therefore, it is necessary to develop a carbon molecular sieve membrane with simple preparation process and good gas separation performance and a preparation method thereof. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention aims to provide a carbon molecular sieve membrane and a preparation method and application thereof. The preparation method improves the pore structure and distribution of the carbon molecular sieve membrane by adding rare earth salts for rare earth coordination modification and carbonization, thereby obtaining a carbon molecular sieve membrane with high gas separation performance.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a carbon molecular sieve membrane, the preparation method comprising the following steps:
[0010] (1) A polymer, an organic solvent and a rare earth salt are mixed to form a film to obtain a polymer film precursor.
[0011] (2) Carbonizing the polymer film precursor to obtain a carbon molecular sieve membrane.
[0012] Preferably, the polymer in step (1) comprises any one of polyamide, polysulfone, polyimide, polybenzimidazole or cellulose acetate, or a combination of at least two thereof, and more preferably comprises polyimide and / or polybenzimidazole.
[0013] Exemplarily, the polyamide includes wholly aromatic polyamide and / or semi-aromatic polyamide; the polysulfone includes any one of bisphenol A type polysulfone, polyaryl sulfone or polyether sulfone, or a combination of at least two of them; the polyimide includes any one of polyetherimide, polyamide-imide or copolymer imide, or a combination of at least two of them; the polybenzimidazole includes any one of triptycene-containing polybenzimidazole, ether polybenzimidazole or isophthalic polybenzimidazole, or a combination of at least two of them; the cellulose acetate includes cellulose diacetate and / or cellulose triacetate.
[0014] Preferably, the polymer in step (1) contains a coordinating group.
[0015] Preferably, the coordinating group includes any one of a carboxyl group, an amino group or an imidazole group, or a combination of at least two of them.
[0016] Preferably, the polybenzimidazole comprises triptycene-containing polybenzimidazole.
[0017] In the present invention, the carbon molecular sieve membrane prepared by using the triptycene-containing polybenzimidazole has a larger free volume, thereby obtaining a carbon molecular sieve membrane with higher gas permeability.
[0018] Preferably, the organic solvent in step (1) includes any one or a combination of at least two of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), toluene, acetone, dichloromethane (CH2Cl2), chloroform (CHCl3) or tetrahydrofuran (THF).
[0019] Preferably, the organic solvent is an aprotic polar solvent, and the aprotic polar solvent includes any one of DMF, DMAc, NMP or DMSO, or a combination of at least two thereof.
[0020] Preferably, based on the total mass of the polymer and the organic solvent as 100%, the mass percentage of the polymer is 1-20% (e.g., 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18% or 20%, etc.), preferably 5-15%.
[0021] Preferably, the rare earth salt in step (1) comprises a rare earth chloride.
[0022] The rare earth salt in step (1) includes any one of gadolinium chloride, terbium chloride, dysprosium chloride, holmium chloride, erbium chloride, thulium chloride, ytterbium chloride, lutetium chloride, scandium chloride or yttrium chloride, or a combination of at least two thereof.
[0023] In the present invention, the composite structure formed by the rare earth ions and the polymer in the rare earth salt is carbonized to improve the pore size and distribution of the carbon molecular sieve membrane, so that the ultramicropore diameter is reduced and the submicropore content is increased.
[0024] Preferably, the molar ratio of the rare earth salt to the repeating unit in the polymer is 0.1-2, for example, 0.1, 0.2, 0.5, 0.8, 1, 1.2, 1.4, 1.5, 1.6, 1.8 or 2, and preferably 0.5-2.
[0025] In the present invention, if the molar ratio of rare earth salt to repeating units in the polymer is too small, the gas separation performance of the obtained carbon molecular sieve membrane will not be significantly improved compared with when no rare earth salt is added. If the molar ratio is too large, the gas separation performance of the carbon molecular sieve membrane will be reduced.
[0026] Preferably, the thickness of the polymer film precursor is 10-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm.
[0027] Preferably, the mixing in step (1) is to dissolve the polymer in an organic solvent to obtain a homogeneous polymer solution, then add a rare earth salt, and stir and dissolve it thoroughly to obtain a homogeneous casting solution.
[0028] Preferably, the film forming in step (1) is to pour the homogeneous casting liquid onto a clean horizontal glass plate and dry it.
[0029] Preferably, the drying temperature is 50-300°C, for example 50°C, 70°C, 80°C, 100°C, 130°C, 150°C, 200°C, 230°C, 250°C, 280°C or 300°C, and the drying time is 6-24h, for example 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h, etc.
[0030] Preferably, the carbonization in step (2) is performed by placing the polymer film precursor in a high-temperature tube furnace and carbonizing it in an atmosphere of inert gas or nitrogen.
[0031] Preferably, the inert gas includes any one of helium or argon.
[0032] Preferably, the inert atmosphere is formed by purging with an inert gas or nitrogen for a long time, and the flow rate of the purging inert gas or nitrogen is 100-1000 mL min -1 , e.g. 100 mL min -1 , 200 mL min -1 、300 mL min -1 、400 mLmin -1 、500 mL min -1 、600 mL min -1 、700 mL min -1 、800 mL min -1 、900 mL min -1 or 1000 mL / min -1 The purging time is 6 to 24 h, for example, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h, etc.
[0033] Preferably, the carbonization temperature in step (2) is 500-1000°C, such as 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C or 1000°C, and the heating rate is 0.1-25°C min -1 , for example 0.1℃min -1 、0.5℃ min -1 、1℃ min -1 、2℃ min -1 、5℃ min -1 、7℃ min -1 、10℃ min-1 、12℃ min -1 、15℃ min -1 、17℃ min -1 、20℃ min -1 or 25℃ min -1 The holding time after reaching the carbonization temperature is 60-600 min, for example, 60 min, 100 min, 150 min, 200 min, 250 min, 300 min, 350 min, 400 min, 450 min, 500 min or 600 min, etc.
[0034] In a second aspect, the present invention provides a carbon molecular sieve membrane, which is prepared by the preparation method described in the first aspect.
[0035] In a third aspect, the present invention provides a use of the carbon molecular sieve membrane as described in the second aspect in a gas purification material.
[0036] Preferably, the gas purification includes purifying helium from natural gas, purifying hydrogen from water gas or purifying hydrogen from synthesis gas.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The present invention adds rare earth salts to the polymer film precursor of the carbon molecular sieve membrane for rare earth coordination modification, and obtains the carbon molecular sieve membrane through carbonization. The preparation process is simple, the pore size and distribution of the carbon molecular sieve membrane are improved, and the obtained carbon molecular sieve membrane has high gas permeability and selectivity, thereby improving the gas separation performance of the carbon molecular sieve membrane. The pure gas permeability of He of the carbon molecular sieve membrane is 13.4~465.4 Barrer, the pure gas permeability of H2 is 10.5~858.1 Barrer, the pure gas permeability of N2 is 0.1~15.9 Barrer, the pure gas permeability of CH4 is 0.08~11.3 Barrer, the gas selectivity of He / CH4 is 28~168, the gas selectivity of He / N2 is 20~134, the gas selectivity of H2 / CH4 is 32~453, and the gas selectivity of H2 / N2 is 23~116, and the gas separation performance is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is an infrared spectrum of the carbon molecular sieve membrane provided in Example 1;
[0040] Figure 2 The Raman spectrum of the carbon molecular sieve membrane provided in Example 2;
[0041] Figure 3This is a graph showing the relationship between the pure gas separation performance of the carbon molecular sieve membrane provided in Example 3 and the gas molecule diameter. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0043] Example 1
[0044] This embodiment provides a carbon molecular sieve membrane and a preparation method thereof. The preparation method of the carbon molecular sieve membrane is as follows.
[0045] (1) Dissolve triptycene-containing polybenzimidazole (0.6688 g, the molar number of repeating units is 1 mmol, prepared according to CN115703044A) in DMAc (7.8624 g). After complete dissolution, add ytterbium chloride (0.0279 g, 1 mmol) and stir until complete dissolution to obtain a homogeneous casting solution. Pour the solution onto a clean horizontal glass plate and dry it at 150 °C for 12 h to obtain a polymer film precursor.
[0046] (2) Place the polymer film precursor obtained in step (1) in a tube furnace and introduce nitrogen (500 mL / min) -1 ) was purged for 8 h to form an inert atmosphere. Then, the temperature was increased from room temperature to 10 °C min -1 The heating rate was raised to 600°C and kept warm for 300 min. After natural cooling, the carbon molecular sieve membrane was obtained, and the membrane thickness was 30 μm.
[0047] Example 2
[0048] This embodiment provides a carbon molecular sieve membrane and a preparation method thereof. The preparation method of the carbon molecular sieve membrane is as follows.
[0049] (1) A polybenzimidazole containing triptycene (1.3776 g, the molar number of the repeating unit is 2 mmol, prepared according to CN115703044A) was dissolved in NMP (15.4964 g). After complete dissolution, ytterbium chloride (0.0279 g, 1 mmol) was added and stirred until complete dissolution to obtain a homogeneous casting solution, which was poured onto a clean horizontal glass plate and dried at 200 °C for 24 h to obtain a polymer film precursor.
[0050] (2) Place the polymer film precursor obtained in step (1) in a tube furnace and introduce argon gas (300 mL / min) -1 ) was purged for 12 h to form an inert atmosphere. Then, the temperature was increased from room temperature to 2 °C min-1 The heating rate was raised to 700° C. and kept at this temperature for 120 min. After natural cooling, the carbon molecular sieve membrane was obtained, and the membrane thickness was 25 μm.
[0051] Example 3
[0052] This embodiment provides a carbon molecular sieve membrane and a preparation method thereof. The preparation method of the carbon molecular sieve membrane is as follows.
[0053] (1) Dissolve triptycene-containing polybenzimidazole (1.6719 g, the molar number of repeating units is 2.5 mmol, prepared according to CN115703044A) in CHCl3 (9.4741 g). After complete dissolution, add gadolinium chloride (0.0527 g, 5 mmol) and stir until complete dissolution to obtain a homogeneous casting solution. Pour the solution onto a clean horizontal glass plate and dry it at 50 °C for 10 h to obtain a polymer film precursor.
[0054] (2) Place the polymer film precursor obtained in step (1) in a tube furnace and introduce helium (1000 mL / min) -1 ) was purged for 6 h to form an inert atmosphere. Then, the temperature was increased from room temperature to 20 °C min -1 The heating rate was raised to 800° C. and kept at this temperature for 300 min. After natural cooling, the carbon molecular sieve membrane was obtained, and the membrane thickness was 28 μm.
[0055] Example 4
[0056] This embodiment provides a carbon molecular sieve membrane and a preparation method thereof. The preparation method of the carbon molecular sieve membrane is as follows.
[0057] (1) Polyamide-imide Torlon 4000T (0.8788 g, molar number of repeating units: 2 mmol) was dissolved in DMAc (87.0012 g). After complete dissolution, dysprosium chloride (0.8065 g, 3 mmol) was added and stirred until complete dissolution to obtain a homogeneous casting solution. The solution was cast onto a clean horizontal glass plate and dried at 300 °C for 6 h to obtain a polymer film precursor.
[0058] (2) Place the polymer film precursor obtained in step (1) in a tube furnace and introduce nitrogen (100 mL / min) -1 ) was purged for 24 h to form an inert atmosphere. Then, the temperature was increased from room temperature to 1 °C min -1 The heating rate was raised to 500° C. and kept at this temperature for 600 min. After natural cooling, the carbon molecular sieve membrane was obtained, and the membrane thickness was 10 μm.
[0059] Example 5
[0060] This embodiment provides a carbon molecular sieve membrane and a preparation method thereof. The preparation method of the carbon molecular sieve membrane is as follows.
[0061] (1) Dissolve polyetherimide Ultem 1000 (1.7839 g, the molar number of repeating units is 3 mmol) in DMAc (7.1354 g). After complete dissolution, add holmium chloride (0.0652 g, 0.3 mmol) and stir until complete dissolution to obtain a homogeneous casting solution. Pour the solution onto a clean horizontal glass plate and dry it at 100 °C for 12 h to obtain a polymer film precursor.
[0062] (2) Place the polymer film precursor obtained in step (1) in a tube furnace and introduce helium (800 mL / min) -1 ) was purged for 18 h to form an inert atmosphere. Then, the temperature was increased from room temperature to 25 °C min -1 The heating rate is raised to 1000°C and kept at this temperature for 60 min. After natural cooling, the carbon molecular sieve membrane is obtained, and the membrane thickness is 100 μm.
[0063] Example 6
[0064] This embodiment provides a carbon molecular sieve membrane and a preparation method thereof. The preparation method of the carbon molecular sieve membrane is as follows.
[0065] (1) Dissolve bisphenol A type polysulfone Udel P-3500 (2.2228 g, the molar number of repeating units is 5 mmol) in DMSO (8.8912 g). After complete dissolution, add thulium chloride (0.3216 g, 1.25 mmol) and stir until complete dissolution to obtain a homogeneous casting solution. Pour it onto a clean horizontal glass plate and dry it at 200 °C for 24 h to obtain a polymer film precursor.
[0066] (2) Place the polymer film precursor obtained in step (1) in a tube furnace and introduce argon gas (300 mL / min) -1 ) was purged for 12 h to form an inert atmosphere. Then, the temperature was increased from room temperature to 2 °C min -1 The heating rate was raised to 700° C. and kept at this temperature for 120 min. After natural cooling, the carbon molecular sieve membrane was obtained, and the membrane thickness was 25 μm.
[0067] Example 7
[0068] This embodiment provides a carbon molecular sieve membrane and a preparation method thereof. The preparation method of the carbon molecular sieve membrane is as follows.
[0069] (1) Cellulose triacetate CA 9004-35-7 (2.8800 g, the molar number of repeating units is 10 mmol) was dissolved in CH2Cl2 (11.5200 g). After complete dissolution, lutetium chloride (0.1747 g, 0.8 mmol) was added and stirred until complete dissolution to obtain a homogeneous casting solution. The solution was poured onto a clean horizontal glass plate and dried at 200 °C for 24 h to obtain a polymer film precursor.
[0070] (2) Place the polymer film precursor obtained in step (1) in a tube furnace and introduce argon gas (300 mL / min) -1 ) was purged for 12 h to form an inert atmosphere. Then, the temperature was increased from room temperature to 2 °C min -1 The heating rate was raised to 700° C. and kept at this temperature for 120 min. After natural cooling, the carbon molecular sieve membrane was obtained, and the membrane thickness was 25 μm.
[0071] Comparative Example 1
[0072] This comparative example provides a carbon molecular sieve membrane and a preparation method thereof, which is different from Example 1 only in that ytterbium chloride is not added in step (1), and other conditions are the same as those in Example 1.
[0073] The separation performance of the carbon molecular sieve membranes provided in the examples and comparative examples was tested.
[0074] Pure gas permeability: The gas permeability test adopts the isochoric pressure change method, that is, changing the gas pressure on both sides of the membrane, and realizing the process of gas permeation through the membrane by pressure drive. When gas molecules pass through the membrane, they follow the dissolution-diffusion mechanism and diffuse from the high concentration (pressure) side through the membrane to the low concentration (pressure) side. After a period of stable operation, Q is defined as the volume of gas diffusion per unit time, Δp is the pressure difference on both sides of the membrane, A is the effective membrane area through which the gas passes, and l is the thickness of the membrane. The gas permeability P is calculated according to the following formula:
[0075] P=Q·l·Δp -1 ·A -1 ,
[0076] The commonly used unit of P is Barrer=1×10 -10 cm 3 ·(STP)·cm·cm -2 ·s -1 cmHg -1 .
[0077] Gas selectivity: Gas selectivity is defined as the ratio of the permeability of a faster-permeating gas A to a slower-permeating gas B: α A / B =P A / P B .
[0078] The test inlet pressure is 100 PSIA and the test temperature is 35°C.
[0079] The test results are shown in Table 1.
[0080] Table 1
[0081]
[0082] According to the test results in Table 1, the carbon molecular sieve membrane provided in Examples 1-7 has a pure gas permeability of He of 13.4~465.4 Barrer, a pure gas permeability of H2 of 10.5~858.1 Barrer, a pure gas permeability of N2 of 0.1~15.9 Barrer, a pure gas permeability of CH4 of 0.08~11.3 Barrer, a gas selectivity of He / CH4 of 28~168, a gas selectivity of He / N2 of 20~134, a gas selectivity of H2 / CH4 of 32~453, a gas selectivity of H2 / N2 of 23~116, and has good gas separation performance.
[0083] The selection of different polymers as precursors, carbonization temperature and the amount of rare earth salt added all affect the gas separation performance of the obtained carbon molecular sieve membrane. Generally speaking, the higher the pyrolysis temperature, the lower the gas permeability and the higher the selectivity. The carbon molecular sieve membrane obtained by using polybenzimidazole containing triptycene as a precursor has higher gas permeability under similar selectivity.
[0084] Figure 1 This is the infrared spectrum of the carbon molecular sieve membrane of Example 1. As can be seen from the figure, the infrared characteristic peak of the polymer disappears, indicating that the carbonization of the polybenzimidazole containing triptycene as a precursor is relatively sufficient. Figure 2 This is the Raman spectrum of Example 2. From the figure, it can be seen that the carbon molecular sieve membrane after carbonization has D peak and G peak which are unique to carbon materials, indicating that the carbonization is complete. Figure 3 3 is a graph showing the relationship between gas permeability and gas molecule diameter in Example 3. From the graph, we can see that as the gas size increases, the gas permeability gradually decreases, indicating that the sieving effect plays a dominant role in the carbon molecular sieve membrane.
[0085] Compared with Example 1, if no rare earth salt is added (Comparative Example 1), the pure gas permeability of He, the pure gas permeability of H2, the pure gas permeability of N2 and the pure gas permeability of CH4 are improved, but the gas selectivity of He / CH4 decreases by 30%, the gas selectivity of He / N2 decreases by 29%, the gas selectivity of H2 / CH4 decreases by 31%, the gas selectivity of H2 / N2 decreases by 22%, and the gas separation performance decreases.
[0086] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a carbon molecular sieve membrane, characterized in that: The preparation method comprises the following steps: (1) 0.8788 g of polyamide-imide Torlon 4000T (the molar number of repeating units is 2 mmol), 87.0012 g of organic solvent DMAc and 0.8065 g of rare earth salt dysprosium chloride (3 mmol) were mixed and formed into a film to obtain a polymer film precursor; (2) Carbonizing the polymer film precursor to obtain a carbon molecular sieve membrane.
2. The preparation method according to claim 1, characterized in that: The thickness of the polymer film precursor is 10-100 μm.
3. The preparation method according to claim 1, characterized in that: The mixing in step (1) is to dissolve 0.8788 g of polyamideimide Torlon 4000T with a molar number of repeating units of 2 mmol in 87.0012 g of DMAc to obtain a homogeneous polymer solution, and then add 0.8065 g, 3 mmol of dysprosium chloride, and stir thoroughly to obtain a homogeneous casting solution.
4. The preparation method according to claim 3, characterized in that: The film forming in step (1) is to pour the homogeneous film casting liquid onto a clean horizontal glass plate and dry it.
5. The preparation method according to claim 4, characterized in that: The drying temperature is 50-300° C. and the drying time is 6-24 h.
6. The preparation method according to claim 1, characterized in that: The carbonization in step (2) is to place the polymer film precursor in a high-temperature tube furnace and carbonize it in a nitrogen atmosphere.
7. The preparation method according to claim 6, characterized in that: The nitrogen atmosphere was formed by long-term nitrogen purge, and the flow rate of the purge nitrogen was 100 mL min -1 The purge time is 24 h.
8. The preparation method according to claim 1, characterized in that: The carbonization temperature in step (2) is 500°C, and the heating rate is 1°C min -1 After reaching the carbonization temperature, the insulation time is 600 min.
9. A carbon molecular sieve membrane, characterized in that: The carbon molecular sieve membrane is prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the carbon molecular sieve membrane as claimed in claim 9 in gas purification materials.
11. Use of the carbon molecular sieve membrane in gas purification materials according to claim 10, characterized in that: The gas purification includes purifying helium from natural gas, purifying hydrogen from water gas or purifying hydrogen from synthesis gas.
Citation Information
Patent Citations
Supported composite carbon molecular sieve membrane
CN105621389A
Ultra-selective carbon molecular sieve membranes and methods of making
CN107635646A
Carbon molecular sieve membrane with improved permeability and selectivity as well as preparation method and application thereof
CN112044273A
Structure, preparation method and application of heterocyclic polybenzimidazole gas separation membrane
CN115703044A
Metal organic framework film with polymer as ligand
CN108114696A