A method for manufacturing military map paper
By mixing northern bleached softwood kraft pulp and southern bleached hardwood kraft pulp in proportion, and adding auxiliary materials such as polyamide epichlorohydrin resin, the problems of folding endurance and mildew resistance of map paper in high-humidity environments are solved. It achieves high-quality printing effects and environmental safety, and improves the competitiveness and economic benefits of the product.
Patent Information
- Application Number
- CN202310655871.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-06-05
AI Technical Summary
Existing map paper has low folding resistance in high-humidity environments, poor resistance to moisture deformation, and is prone to mildew and rot. It is also harmful to the human body and the environment. The printing clarity is not high, and the dry paper produced during the papermaking process is difficult to break. Solve and reuse.
The northern bleached softwood kraft pulp and the southern bleached hardwood kraft pulp are mixed in proportion, and auxiliary materials such as polyamide epichlorohydrin resin are added. Through beating, compound pressing, drying and surface sizing, it is made with high folding resistance. , wet strength and surface strength military map paper to ensure accurate printing overprint and resistance to mildew and rot.
It improves the folding resistance, wet strength and surface strength of the map paper, ensures good printing effect, prevents mildew and rot, solves the problem of dry damaged paper fragmentation, improves the environmental and human safety of the product, and meets the requirements of military map paper. High quality requirements and brought economic benefits.
Smart Images

Figure BDA0004266894020000101 
Figure BDA0004266894020000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of papermaking technology, and in particular relates to a method for manufacturing military map paper. Background Art
[0002] Map paper is mainly used for printing topography, landform, hydrology, traffic wall maps and map books, etc. For example, when used for printing military maps, it has high requirements on the folding resistance, wet strength, surface strength, smoothness, dust resistance and shrinkage rate of the paper. It is required to obtain printed materials with accurate overprint, clear lines, dense dots, correct proportions and small wet deformation, and it must be anti-moth and anti-mildew and rot. The product specifications include 590mm*940mm and 620mm*940mm flat specifications.
[0003] At present, the map papers on the market mainly come from some papermaking companies that use non-wood fiber or high-yield pulp to make paper, and add fluorescent brighteners to the pulp. When treating the surface of the paper, fluorescent agents or volatile organic compounds are added. This kind of map paper has low folding resistance, poor resistance to moisture deformation, inaccurate overprinting, low printing clarity, is prone to moths, and is prone to mildew and rot in a humid environment, and poses certain hazards to the human body and the environment. Summary of the invention
[0004] In view of the above problems, the present invention provides a method for manufacturing military map paper. The present invention develops and manufactures a military map paper. The manufacturing process can improve the folding resistance, wet strength and surface strength of the map paper, improve the anti-moth, mildew and decay resistance, make the paper printing overprint accurate, the lines clear, the dots dense, the proportions correct and the wet deformation small, the durability is good, and will not cause harm to the environment and human health, which is conducive to printing military maps and other applications.
[0005] The present invention provides a method for manufacturing a military map paper, comprising the following steps:
[0006] S1. Beating northern bleached softwood kraft pulp, and controlling the beating degree to be 43-47°SR;
[0007] The southern bleached hardwood kraft pulp is pulped, and the beating degree is controlled to be 38-42°SR;
[0008] S2, mixing the northern bleached softwood kraft pulp and the southern bleached hardwood kraft pulp according to the mass percentage: 25-30% of northern bleached softwood kraft pulp and 70-75% of southern bleached hardwood kraft pulp;
[0009] S3, adding auxiliary materials to the prepared slurry to carry out wet sheet papermaking; the auxiliary materials include: internal sizing agent, retention aid, cationic starch, filler and polyamide epichlorohydrin resin;
[0010] S4, sequentially subjecting the obtained wet paper sheet to composite pressing, front-stage drying, surface sizing treatment containing an antibacterial agent, back-stage drying, and calendering and finishing to obtain a military map paper;
[0011] The weight of the military map paper is 78-85 g / m 2 , the aspect ratio of breaking length is less than 1.5, and the transverse wet strength retention rate is above 15%.
[0012] Preferably, in step S1, the northern bleached softwood kraft pulp is a mixed pulp of Canadian hemlock, black spruce and white pine, and the pulping concentration is controlled at 4.0-4.5%.
[0013] Preferably, in step S1, the southern bleached hardwood kraft pulp is made from acacia, and the pulping concentration is controlled at 3.5-4.0%.
[0014] Preferably, in step S3, the auxiliary materials specifically include: 30-35 kg / ton of paper of internal sizing agent, 0.5-1.0 kg / ton of paper of retention aid, 8-10 kg / ton of paper of cationic starch, 120-150 kg / ton of paper of filler, and 25-30 kg / ton of paper of polyamide epichlorohydrin resin.
[0015] Preferably, in step S3, the internal sizing agent is AKD emulsion, and the paper absorbency is controlled at 15-18 g / m 2 The retention aid is cationic polyacrylamide, which controls the white water concentration under the screen to 0.2-0.25%; the filler is PCC.
[0016] Preferably, in step S3, the slurry is mixed with the added auxiliary materials and diluted to a concentration of 2.5-3.5%, and then the slurry is desanded and diluted by the screening system. The slurry concentration on the screen is 0.8-0.9%, the opening of the headbox lip is controlled to be 11.0-11.5 mm, the headbox pressure head is controlled to be 57.0-58.0 Kpa, and wet paper sheet making is completed in the screen part.
[0017] Preferably, in step S4, the formulation of the surface sizing treatment containing an antimicrobial agent comprises a surface sizing agent, a sizing starch and an antimicrobial agent; the surface sizing agent is a styrene ester copolymer, the sizing starch is enzyme-converted cassava starch, the antimicrobial agent is a biguanide, and the surface sizing treatment amount is 4.0-4.5 g / m 2 .
[0018] Preferably, in step S4, the specific process of calendering finishing includes: a first calendering pressure of 65-75 kg / cm, and a second calendering pressure of 40-50 kg / cm.
[0019] Preferably, the manufacturing method further comprises: sending the dry damaged paper generated in the papermaking process to a pressure high-consistency disintegration device for disintegration, and then returning it for pulping.
[0020] Preferably, the concentration in the pressure high-concentration crushing equipment is controlled at 15-18%, the pH value is adjusted to 4-5, the temperature is controlled at 85-90° C., the treatment time is 1-2 hours, and the dry damaged paper to be treated is placed for no more than 6 hours.
[0021] Compared with the prior art, the present invention mainly starts from the research of fiber raw materials, mixes the northern bleached softwood sulfate pulp (NBSK) and the southern bleached hardwood sulfate pulp (SBHK) in proportion, and uses functional chemical additives such as polyamide epichlorohydrin resin and antibacterial agent to make paper, and the aspect ratio of the breaking length is within 1.5. The map paper prepared is used as military map paper (quantity 78-85g / m 2 ), the paper is fine, has high folding resistance, high wet strength, high surface strength, accurate printing overprint, clear lines, dense dots, correct proportions and small wet deformation; in a high humidity environment, the map paper is not easy to break, resistant to rubbing and folding, and resistant to mildew, rot and insects during storage, which can meet people's high usage requirements and quality requirements for military map paper.
[0022] The present invention solves the technical problems that map paper is easy to break, mold and rot, and is eaten by insects during storage in a high humidity environment, and further solves the problem that dry damaged paper generated in the process of copying military map paper is difficult to break and reuse. It not only improves the competitiveness of the enterprise and lays a foundation for the long-term and healthy development of the enterprise, but also brings economic benefits (this kind of military map paper is a special paper with a good selling price and high profit, and the product price is more than 10,000 yuan / ton). DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with specific embodiments. The description in this section is only exemplary and explanatory and should not have any limiting effect on the scope of protection of the present invention.
[0024] The present invention provides a method for manufacturing a military map paper, comprising the following steps:
[0025] S1. Beating northern bleached softwood kraft pulp, and controlling the beating degree to be 43-47°SR;
[0026] The southern bleached hardwood kraft pulp is pulped, and the beating degree is controlled to be 38-42°SR;
[0027] S2, mixing the northern bleached softwood kraft pulp and the southern bleached hardwood kraft pulp according to the mass percentage: 25-30% of northern bleached softwood kraft pulp and 70-75% of southern bleached hardwood kraft pulp;
[0028] S3, adding auxiliary materials to the prepared slurry to carry out wet sheet papermaking; the auxiliary materials include: internal sizing agent, retention aid, cationic starch, filler and polyamide epichlorohydrin resin;
[0029] S4, sequentially subjecting the obtained wet paper sheet to composite pressing, front-stage drying, surface sizing treatment containing an antibacterial agent, back-stage drying, and calendering and finishing to obtain a military map paper;
[0030] The weight of the military map paper is 78-85 g / m 2 , the aspect ratio of breaking length is less than 1.5, and the transverse wet strength retention rate is above 15%.
[0031] In view of the above-mentioned problems existing in the prior art, the purpose of the present invention is to provide a method for manufacturing military map paper, improve the folding resistance, wet strength and surface strength of the map paper, so that the printing overprint is accurate, the lines are clear, the dots are dense, the proportions are correct and the wet deformation is small, the whiteness of the military map paper is improved, and the mildew and antibacterial properties are improved. The problem of yellowing of map paper can be solved, and the technical problems that map paper is easy to break, mildew and rot in a high humidity environment, and is infested by insects during storage can be solved. The problem of slurry pump blockage and paper fragments appearing on the paper surface when dry damaged paper is shredded and reused can also be solved, thereby improving the competitiveness of the enterprise, laying a foundation for the long-term and healthy development of the enterprise, and bringing economic benefits.
[0032] To achieve the above purpose, the technical solution for manufacturing map paper adopted by the present invention is: it includes mixing the pulped northern bleached softwood sulfate pulp (NBSK) and southern bleached hardwood sulfate pulp (SBHK) in proportion, adding auxiliary materials, removing sand (pulping, removing slag and degassing), screening (which can be carried out by pressure screen), pulp dilution, wet paper sheet papermaking on the wire, composite pressing, front-stage drying, paper sheet sizing surface treatment, back-stage drying, calendering and curling process steps.
[0033] In an embodiment of the present invention, the northern bleached softwood kraft pulp is a mixture of Canadian hemlock, black spruce and white pine, and is pulped by the kraft process; the wet breaking length of the base paper is 30-40% higher than that of the base paper made from other softwood pulps, and the ISO brightness of the pulp can be 88.5-89.5%, such as ISO brightness 89%. The three northern softwoods of Canadian hemlock, black spruce and white pine are pulped by the kraft process, and the original pulp breaking length is excellent, which is 20-25% higher than the local bleached softwood pulp, especially the wet breaking length is 30-40% higher than other softwood pulps, and the pulping yield is high, at 49-50%. Through pulping, the growth of physical strength indicators is also very excellent. At a beating degree of 40°SR, the pulp breaking length can reach 9.0-9.5km, the folding endurance is ≥2200 times, and the wet breaking length is 0.45-0.55km. At the same time, the northern bleached softwood kraft pulp is reasonably beaten, and the beating concentration can be controlled at 4.0-4.5%. The beating degree is preferably controlled at 45±2°SR.
[0034] Furthermore, the southern bleached hardwood kraft pulp is preferably made from acacia, and the paper is fine, flat, and smooth, and the ISO whiteness of the pulp is preferably 87.5-88.5%, such as ISO whiteness 88%. The southern bleached hardwood kraft pulp can be pulped, and the pulping concentration is controlled at 3.5-4.0%, and the beating degree is controlled to be 40±2°SR. In the present invention, the fiber raw materials are northern bleached softwood (mixed pulping of hemlock, black spruce, and white pine) kraft pulp, and southern bleached hardwood (acacia) kraft pulp. The combination of these two fiber raw materials can improve the physical strength, fineness, folding and rubbing resistance of military map paper, high paper whiteness and not easy to yellow, and good printing effect.
[0035] In the embodiment of the present invention, the pulped northern bleached softwood kraft pulp (NBSK) and southern bleached hardwood kraft pulp (SBHK) are mixed according to 25-30% by mass percentage of northern bleached softwood kraft pulp and 70-75% by mass percentage of southern bleached hardwood kraft pulp.
[0036] In the embodiment of the present invention, the prepared slurry is added with auxiliary materials, and wet sheet papermaking is performed through papermaking equipment. The auxiliary materials include: internal sizing agent, retention aid, cationic starch, filler and polyamide epichlorohydrin resin. Specifically, the auxiliary materials are added by a metering pump: 30-35kg / ton of paper of internal sizing agent, 0.5-1.0kg / ton of paper of retention aid, 8-10kg / ton of paper of cationic starch, 120-150kg / ton of paper of filler, and 25-30kg / ton of paper of polyamide epichlorohydrin resin. The slurry and the added auxiliary materials are mixed evenly and diluted, and then the slurry is desanded and diluted by the screening system. The slurry concentration on the net is preferably 0.8-0.9%, and the opening of the headbox lip can be controlled to be 11.0-11.5mm. The diluted slurry is dehydrated and formed into wet paper sheets in the net part to complete the wet sheet papermaking.
[0037] As a preferred embodiment, the internal sizing agent is alkyl ketene dimer AKD emulsion, and the paper absorbency is controlled at 15-18g / m 2(60 seconds). The AKD emulsion generally selected has a solid content of 15%, a pH value of 3-4, and a particle size of 0.5-2.0 microns. The retention aid is preferably a cationic polyacrylamide (e.g., its molecular weight is 8 million, the cationic concentration is 20-30%, the dissolution time is ≤60 minutes, and the dissolution concentration is 0.2-0.28%), and the white water concentration under the screen is controlled to be 0.2-0.25%. The filler is preferably precipitated calcium carbonate (PCC), specifically PCC with an ISO whiteness of 90%, and the slurry concentration on the screen can be 0.8-0.9%; in addition, the median particle size of the PCC filler can be 2.0-2.5 microns, the pH value can be 8-9, and the solid content can be 20-25%. The degree of substitution of the cationic starch in the auxiliary material can be 0.02-0.03, its solid content is 10%, and the room temperature viscosity is 200-400mpas. The main function of the polyamide epichlorohydrin resin is to improve the wet strength. The specific room temperature viscosity can be 15-25mpas, the solid content is 12-13%, and the pH value is 3-5. All of the above are commercially available products. In addition, the opening of the headbox lip is preferably controlled to be 11.0-11.5mm, and the headbox pressure head is controlled to be 57.0-58.0Kpa; the optimized pulp-to-net speed ratio is 1.00-1.002.
[0038] The wet paper sheets obtained in the embodiment of the present invention are fed into the press section for composite pressing, and the paper sheet dryness can be 40-45%, and then enter the front-stage drying cylinder for drying until the paper sheet moisture content is less than 8%; then, the front-dried paper sheets are subjected to sizing surface treatment containing an antibacterial agent, and then enter the back-stage drying cylinder for drying, at which time the paper sheet moisture content can be controlled at 6.5-7.0%. The optimized composite pressing key control parameters include: a press pressure of 5.0kg / cm 3 , the second pressure operating pressure is 85N / mm, and the third pressure operating pressure is 115N / mm.
[0039] In an embodiment of the present invention, the surface sizing treatment formula containing an antibacterial agent includes a surface sizing agent, sizing starch and an antibacterial agent, and the surface is micro-coated, and the surface sizing treatment amount is 4.0-4.5g / m 2 . In the surface micro-coating formula, the surface sizing agent is preferably a styrene ester copolymer, the sizing starch is preferably enzyme-converted cassava starch, and the antibacterial agent is preferably a biguanide, and commercially available products can be used. When applying the surface sizing, the sizing starch, styrene ester copolymer, and antibacterial agent can be compounded in a mass ratio of (85-95): (3-8): (2-7); after compounding at room temperature, the viscosity of the sizing material is 10-30mpas, and the solid content is preferably 8-15%.
[0040] In the method for manufacturing the map paper of the embodiment of the present invention, polyamide epichlorohydrin resin is added to the pulp, and styrene ester copolymer surface sizing agent, enzyme-converted cassava starch, and biguanide antibacterial agent are added to the surface micro-coating, which is beneficial to improving the surface strength and wet strength, so that the printing is clear, the dots are dense, the overprint is accurate, and it can prevent moths, mildew and decay.
[0041] The dried paper sheets are sent to the calendering area for finishing to achieve the desired smoothness of the paper. In addition, the dry damaged paper produced during the papermaking process of the map paper of the embodiment of the present invention is sent to the high-consistency shredder for full decomposition, and then re-enters the pulping system to prepare pulp for papermaking.
[0042] In the embodiment of the present invention, the calendering finishing is to perform multiple line pressing in the calendering area to improve the smoothness of the paper; the specific process preferably includes: the first line pressing pressure is 65-75kg / cm, and the second line pressing pressure is 40-50kg / cm. The embodiment of the present invention strictly controls the process parameters such as pulp beating degree, pulp ratio, auxiliary material dosage, web concentration, headbox lip opening, pulp-web speed ratio, composite pressing pressure, drying moisture, calendering pressure, etc., so that the aspect ratio of the breaking length is within 1.5, ensuring that the paper strength and wet-change performance meet the printing and use requirements.
[0043] The dry damaged paper produced in the existing papermaking process produces paper fragments on the paper, which easily leads to poor uniformity and flatness of the map paper. In the preferred embodiment of the present invention, the treatment of the dry damaged paper produced in the papermaking process of the military map paper is mainly to use a pressure high-concentration shredder to shred it, and it can also be combined with a disc grinder to treat the dry damaged paper. The dry damaged paper is completely disintegrated into single fibers and reused to make military map paper. This does not affect the physical strength and flatness of the paper and will not clog the pulp pump. The pressure high-concentration shredder can be used to control the shredding concentration and temperature, and aluminum sulfate can be added to adjust the pH value. Preferably, after 1-1.5 hours of treatment, it is pumped to the pulping system for re-slurrying and papermaking.
[0044] Optimally, the concentration in the pressure high-concentration crushing equipment is controlled at 15-18%; aluminum sulfate can be added to adjust the pH value to 4-5, preferably pH 4.5, and the temperature is controlled at 85-90°C, and the treatment can be carried out for 1-2 hours. The dry damaged paper to be treated should not be placed for more than 6 hours, otherwise the polyamide epichlorohydrin resin will not be fully crushed after curing.
[0045] The manufacturing method of military map paper provided by the present invention overcomes the great manufacturing difficulty. The folding resistance, wet strength and surface strength of the map paper are improved by the process method. The basis weight of the map paper is 78-85g / m 2The aspect ratio of the breaking length is lower than 1.5, and the transverse wet strength retention rate is above 15%; the paper is fine, has high folding resistance, high wet strength and high surface strength, so the printing overprint is accurate, the lines are clear, the dots are dense, the proportions are correct and the wet deformation is small, which meets people's high usage and quality requirements for military map papers, solves the problems of map papers being easy to break, mildew and rot in high humidity environments, and being eaten by insects during storage, and also solves the problems of dry damaged paper being difficult to break and reuse during the copying process of military maps, which has important social and economic significance.
[0046] In order to better understand the technical content of the present invention, the following specific examples are provided to further illustrate the present invention. In the following examples, unless otherwise specified, all are weight ratios; the raw materials used are commercially available and conventional equipment is used.
[0047] Among them, northern bleached softwood kraft pulp is made from Canadian hemlock, black spruce and white pine. Northern bleached softwood kraft pulp: fiber length>2.900 microns, breaking length>9.0km, tear index>12mN.m 2 / g, folding endurance ≥ 2300 times, wet tear length 0.45-0.55km, pulp ISO whiteness 89%. Southern bleached hardwood kraft pulp is made from acacia wood, tear length> 6.5km, tear index> 8.0mN.m 2 / g, and the ISO brightness of the pulp is 88%.
[0048] Among the auxiliary materials, the sizing agent in the slurry is AKD emulsion, with a solid content of 15%, a pH value of 3-4, and a particle size of 0.5-2.0 microns. The retention aid is cationic polyacrylamide, with a molecular weight of 8 million, a cationic concentration of 20-30%, a dissolution time of ≤60 minutes, and a dissolution concentration of 0.2-0.28%. Cationic starch: substitution degree 0.02-0.03, solid content 10%, viscosity 200-400mpas. Polyamide epichlorohydrin resin: viscosity 15-25mpas, solid content 12-13%, pH value: 3-5. PCC filler: median particle size 2.0-2.5 microns, pH value 8-9, solid content 20-25%, ISO whiteness 90%.
[0049] Example 1: 80 grams of military map paper
[0050] A. Rationally beat the northern bleached softwood kraft pulp, and control the pulping concentration at 4.0%. The beating degree is controlled at 40°SR;
[0051] B. Rationally beat the southern bleached hardwood kraft pulp, control the pulping concentration at 3.5%, and the beating degree at 38°SR;
[0052] C. Mix the beaten northern bleached softwood kraft pulp and southern bleached hardwood kraft pulp according to the mass percentage: 25% northern bleached softwood kraft pulp and 75% southern bleached hardwood kraft pulp;
[0053] D. Use a metering pump to add auxiliary materials: 30kg / ton paper of sizing agent, 0.5kg / ton paper of retention aid, 8kg / ton paper of cationic starch, 150kg / ton paper of filler, 25kg / ton paper of polyamide epichlorohydrin resin, mix evenly and dilute to a concentration of 2.5%, then remove sand and dilute with refined pulp through a screening system. At this time, the pulp concentration on the net is 0.84%, the opening of the headbox lip is controlled to be 11.5mm, and the pulp-to-net speed ratio is 1.000; the diluted pulp is dehydrated on the wire to form a wet paper sheet;
[0054] E. After the wet paper enters the pressing section for compound pressing, the dryness of the paper is 40%, and then enters the front drying cylinder for drying until the moisture content of the paper is 7%; the key control parameters of compound pressing are: the first pressing pressure is 5.0kg / cm 3 , second pressure operating pressure 85N / mm, third pressure operating pressure 115N / mm;
[0055] F. The front drying paper sheet is treated with sizing surface and then enters the back drying cylinder for drying. At this time, the moisture content of the paper sheet is 7.0%; in the surface micro-coating formula: the surface sizing agent is a styrene ester copolymer, the surface sizing starch is enzyme-converted cassava starch, the antibacterial agent is biguanide, the dosage is 3kg / ton of paper, and the surface sizing amount is 4.0g / m 2 The sizing starch, styrene ester copolymer and antimicrobial agent are compounded in a mass ratio of (85-95): (3-8): (2-7); the viscosity of the compounded sizing material at room temperature is 10-30mpas and the solid content is 8-15%;
[0056] G. The dry paper sheets are sent to the calendering area for paper finishing. After reaching the ideal paper smoothness, they are curled to make military map paper; the first pressing line pressure is 65kg / cm, and the second pressing line pressure is 40kg / cm;
[0057] H. The dry damaged paper produced in the process of making map paper enters the high-concentration shredder to be fully disintegrated, and then re-enters the pulping system to prepare pulp for papermaking. The concentration of the high-concentration shredder is 15%, and aluminum sulfate is added to adjust the pH to 4.5. The temperature is controlled at 85°C and treated for 1 hour. The treated dry damaged paper should be placed for no more than 6 hours.
[0058] Example 2: 80g military map paper
[0059] A. Rationally beat the northern bleached softwood kraft pulp, and control the pulping concentration at 4.5%. The beating degree is controlled at 46°SR;
[0060] B. beating southern bleached hardwood kraft pulp, controlling the pulping concentration at 4.0% and the beating degree at 42°SR;
[0061] C. Mix the beaten northern bleached softwood kraft pulp and southern bleached hardwood kraft pulp according to the mass percentage: 30% northern bleached softwood kraft pulp and 70% southern bleached hardwood kraft pulp;
[0062] D. Use a metering pump to add auxiliary materials: sizing agent 35kg / ton paper, retention aid 1.0kg / ton paper, cationic starch 10kg / ton paper, filler 130kg / ton paper, polyamide epichlorohydrin resin 30kg / ton paper, mix and dilute evenly to a concentration of 3.5%, then remove sand and dilute with refined pulp through a screening system. At this time, the pulp concentration on the net is 0.9%, the headbox lip opening is controlled to 11.0mm, and the pulp-to-net speed ratio is 1.002; the diluted pulp is dehydrated on the wire to form a wet paper sheet;
[0063] E. After the wet paper enters the pressing section for compound pressing, the dryness of the paper is 45%, and then enters the front drying cylinder for drying to a moisture content of 6.0%; the key control parameters of compound pressing: the first pressing pressure is 5.5kg / cm 3 , second pressure operating pressure 90N / mm, third pressure operating pressure 125N / mm;
[0064] F. The front drying paper sheet is treated with sizing surface and then enters the back drying cylinder for drying. At this time, the moisture content of the paper sheet is 6.5%; in the surface micro-coating formula: the surface sizing agent is a styrene ester copolymer, the surface sizing starch is enzyme-converted cassava starch, the antibacterial agent is biguanide, the dosage is 4kg / ton of paper, and the surface sizing amount is 4.5g / m 2 The sizing starch, styrene ester copolymer and antimicrobial agent are compounded in a mass ratio of (85-95): (3-8): (2-7); the viscosity of the compounded sizing material at room temperature is 10-30mpas and the solid content is 8-15%;
[0065] G. The dry paper sheets are sent to the calendering area for paper finishing. After reaching the ideal paper smoothness, they are curled to make military map paper; the first pressing line pressure is 75kg / cm, and the second pressing line pressure is 50kg / cm;
[0066] H. The dry damaged paper produced in the process of making map paper enters the high-concentration shredder to be fully disintegrated, and then re-enters the pulping system to prepare pulp for papermaking. The concentration of the high-concentration shredder is 18%, and aluminum sulfate is added to adjust the pH to 4.0. The temperature is controlled at 90°C and treated for 1.5 hours. The treated dry damaged paper should be placed for no more than 6 hours.
[0067] Comparative Example 1: 80g map paper
[0068] A. Rationally beat the local pine kraft pulp, and control the pulping concentration at 4.0%. The beating degree is controlled to 40°SR; local bleached pine kraft pulp: fiber length>2.200 microns, breaking length>7.0km, tear index>9.0mN.m 2 / g, whiteness 88.5-89.5%.
[0069] B. Rationally beat the acacia bleached kraft pulp, control the pulping concentration at 3.5%, and the beating degree at 38°SR;
[0070] C. Mix the beaten local Masson pine kraft pulp and acacia kraft pulp according to the mass percentage: 25% of local Masson pine bleached kraft pulp and 75% of acacia kraft pulp;
[0071] D. Use a metering pump to add auxiliary materials: sizing agent 30kg / ton paper, retention aid 0.5kg / ton paper, cationic starch 8kg / ton paper, filler 150kg / ton paper, polyamide epichlorohydrin resin 25kg / ton paper, mix evenly and dilute to a concentration of 2.5%, then remove sand and dilute with refined pulp through a screening system. At this time, the pulp concentration on the net is 0.84%, the headbox lip opening is controlled to 11.5mm, and the pulp-to-net speed ratio is 1.000; the diluted pulp is dehydrated on the wire to form a wet paper sheet;
[0072] E. After the wet paper enters the pressing section for compound pressing, the dryness of the paper is 40%, and then enters the front drying cylinder for drying until the moisture content of the paper is 7%; the key control parameters of compound pressing are: the first pressing pressure is 5.0kg / cm 3 , second pressure operating pressure 85N / mm, third pressure operating pressure 115N / mm;
[0073] F. The front drying paper sheet is treated with sizing surface, and then enters the back drying cylinder for drying. At this time, the moisture content of the paper sheet is 7.0%; in the surface micro-coating formula: the surface sizing agent is a styrene ester copolymer, the surface sizing starch is enzyme-converted cassava starch, the antibacterial agent is biguanide, the dosage is 3kg / ton of paper, and the surface sizing amount is 4.0-4.5g / m 2 ; One pressing line pressure is 65kg / cm, the other pressing line pressure is 40kg / cm;
[0074] G. The dry paper leaves are sent to the calendering area for paper finishing. After reaching the ideal paper smoothness, they are curled to make military map paper;
[0075] H. The dry damaged paper produced in the process of making map paper enters the high-concentration shredder to be fully disintegrated, and then re-enters the pulping system to prepare pulp for papermaking. The concentration of the high-concentration shredder is 15%, and aluminum sulfate is added to adjust the pH to 4.5. The temperature is controlled at 85°C and treated for 1 hour. The treated dry damaged paper should be placed for no more than 6 hours.
[0076] The qualities of the map papers obtained in Example 1 (Example 1), Example 2 (Example 2), and Comparative Example 1 (Example 3) are shown in Table 1 below:
[0077] Table 1 Performance quality of map paper manufactured by the method of the embodiment of the present invention
[0078]
[0079]
[0080] Compared with ordinary paper map paper, military map paper has the following characteristics: 1) It has high folding resistance, high wet strength and good surface strength. It is easy to use, can be folded and rubbed at will, and has accurate printing and overprinting, clear lines, dense dots, correct proportions and small wet deformation. 2) It is safer and has a wide range of applications. The paper does not contain fluorescent brighteners, and the surface micro-coating does not contain fluorescent agents or volatile organic compounds, which will not cause harm to the environment and human health. 3) It has the functions of preventing moths, corrosion and mildew.
[0081] It can be seen from Table 1 above that the various physical indicators of the paper prepared in Example 1 and Example 2 can meet the quality requirements of military map paper, while the longitudinal and transverse wet tear lengths of Example 3 do not meet the requirements. After color printing, the paper prepared in Examples 1-2 of the present invention has a black solid density of 1.5, a yellow solid density of 1.3, and a blue solid density of 1.3 on the printed surface, and the overprint error of any two colors is ≤0.05mm.
[0082] In summary, the process steps of the military map paper described in the embodiment of the present invention include: mixing the NBSK and SBHK after pulping in proportion, adding auxiliary materials, and then undergoing pulping, wet paper sheet making in the mesh, composite pressing, front-stage drying, sizing pressing, back-stage drying, calendering and curling. Through the manufacturing method of the present invention, the folding resistance, wet strength and surface strength of the map paper can be improved, and the lateral expansion rate of the map paper can be reduced. The printing overprint is accurate, the lines are clear, the dots are dense, the proportions are correct, and the wet deformation is small. The problem that paper is easy to mold and rot in harsh environments is solved, and the technical problem of inaccurate overprinting due to the large lateral expansion rate of paper is solved. The problem that the printing lines are unclear, the paper is not delicate, and the paper is easy to yellow due to unreasonable pulp beating degree and pulp structure is solved. The problem that the dry damaged paper is difficult to handle due to the high wet strength of the paper, and the paper surface has uneven paper fragments is solved. The rubbing resistance, folding resistance and water resistance of the paper are also enhanced, which is conducive to printing military maps.
[0083] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0084] This article uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. The above is only a preferred implementation of the present invention. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, ordinary technicians in this technical field can make several improvements, modifications or changes without departing from the principles of the present invention, and can also combine the above technical features in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the inventive concept and technical solution to other occasions without improvement, should be regarded as the protection scope of the present invention.
Claims
1. A method for manufacturing a military map paper, characterized in that: The following steps are involved: S1. Beating northern bleached softwood kraft pulp, with the beating degree controlled at 43-47°SR; the northern bleached softwood kraft pulp is a mixed pulp of Canadian hemlock, black spruce and white pine, with the beating concentration controlled at 4.0-4.5%; Beating southern bleached hardwood kraft pulp, the beating degree of which is controlled to be 38-42°SR; the southern bleached hardwood kraft pulp is made from acacia wood, and the beating concentration is controlled to be 3.5-4.0%; S2, mixing the northern bleached softwood kraft pulp and the southern bleached hardwood kraft pulp according to the mass percentage: 25-30% of northern bleached softwood kraft pulp and 70-75% of southern bleached hardwood kraft pulp; S3, adding auxiliary materials to the prepared slurry to carry out wet sheet papermaking; the auxiliary materials include: internal sizing agent, retention aid, cationic starch, filler and polyamide epichlorohydrin resin, the room temperature viscosity of the polyamide epichlorohydrin resin is 15-25mPa.s, and the solid content is 12-13%; S4, sequentially subjecting the obtained wet paper sheets to composite pressing, front-stage drying, surface sizing treatment containing an antibacterial agent, back-stage drying, and calendering finishing to obtain military map paper; the preparation method also includes: sending the dry damaged paper generated during the papermaking process to a pressure high-concentration crushing device for decomposition, and then returning it for pulping; The weight of the military map paper is 78-85 g / m 2 , the aspect ratio of breaking length is less than 1.5, and the transverse wet strength retention rate is above 15%.
2. The method for manufacturing a military map sheet according to claim 1, characterized in that: In step S3, the auxiliary materials specifically include: 30-35 kg / ton of paper of internal sizing agent, 0.5-1.0 kg / ton of paper of retention aid, 8-10 kg / ton of paper of cationic starch, 120-150 kg / ton of paper of filler, and 25-30 kg / ton of paper of polyamide epichlorohydrin resin.
3. The method for manufacturing a military map sheet according to claim 2, characterized in that: In step S3, the internal sizing agent is AKD emulsion, and the paper absorbency is controlled at 15-18 g / m 2 The retention aid is cationic polyacrylamide, which controls the white water concentration under the screen to 0.2-0.25%; the filler is PCC.
4. The method for manufacturing a military map sheet according to claim 2, characterized in that: In step S3, the slurry is mixed with the added auxiliary materials and diluted to a concentration of 2.5-3.5%, and then the slurry is desanded and diluted by the screening system. The slurry concentration on the screen is 0.8-0.9%, the opening of the headbox lip is controlled to be 11.0-11.5mm, and the headbox pressure head is controlled to be 57.0-58.0Kpa, and wet paper sheet making is completed in the screen part.
5. The method for manufacturing a military map sheet according to claim 1, characterized in that: In step S4, the formula of the surface sizing treatment containing an antimicrobial agent includes a surface sizing agent, a sizing starch and an antimicrobial agent; the surface sizing agent is a styrene ester copolymer, the sizing starch is enzyme-converted cassava starch, the antimicrobial agent is a biguanide, and the surface sizing treatment amount is 4.0-4.5 g / m 2 .
6. The method for manufacturing a military map sheet according to claim 1, characterized in that: In step S4, the specific process of calendering finishing includes: a first calendering pressure of 65-75 kg / cm, and a second calendering pressure of 40-50 kg / cm.
7. A method for manufacturing a military map sheet according to any one of claims 1 to 6, characterized in that: The concentration in the pressure high-concentration crushing equipment is controlled to be 15-18%, the pH value is adjusted to 4-5, the temperature is controlled at 85-90° C., the treatment time is 1-2 hours, and the dry damaged paper to be treated is not more than 6 hours.